CN108004667A - 一种环保经编麂皮绒面料生产工艺 - Google Patents
一种环保经编麂皮绒面料生产工艺 Download PDFInfo
- Publication number
- CN108004667A CN108004667A CN201810038928.7A CN201810038928A CN108004667A CN 108004667 A CN108004667 A CN 108004667A CN 201810038928 A CN201810038928 A CN 201810038928A CN 108004667 A CN108004667 A CN 108004667A
- Authority
- CN
- China
- Prior art keywords
- grey cloth
- speed
- production technology
- face fabric
- warp
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
本发明公开了一种环保经编麂皮绒面料生产工艺,依次包括如下步骤:白坯布的织造、白坯布起毛、起毛面料定型、起毛面料染色、柔软处理、磨毛定型、打卷包装。本发明所涉及的一种环保经编麂皮绒面料生产工艺,底纱所使用的原料为54D/24F的FDY,绒纱所使用的原料为75D/488F的DTY,使用白坯布在经过拉毛、定型、染色、剪毛和定型后,能够形成麂皮绒的效果。在本发明中并没有使用碱对白坯布进行处理来形成麂皮绒效果,避免了在污水处理中碱的影响,既减少了生产成本,还避免了碱处理所带来的影响。
Description
技术领域
本发明涉及经编麂皮绒面料生产技术领域,尤其是一种环保经编麂皮绒面料生产工艺。
背景技术
在经编麂皮绒的生产工艺中,使得面料表面产生麂皮是需要用碱对纱线处理,使得面料表面形成麂皮的效果。在这种处理工艺中,使用了强碱,会对环境造成污染。
发明内容
本发明的目的是提供一种环保经编麂皮绒面料生产工艺,能够不使用碱对面料进行处理,就可以实现面料麂皮的效果。
为解决上述技术问题,本发明的目的是这样实现的:
本发明所涉及的一种环保经编麂皮绒面料生产工艺,依次包括如下步骤:
步骤A、白坯布的织造:底纱所使用的原料为54D/24F的FDY,绒纱所使用的原料为75D/488F的DTY,白坯布的纬密为26.5针每厘米;
步骤B、白坯布起毛:采用3组12辊将白坯布进行起毛处理,车速为25米;
步骤C、起毛面料定型:定型温度为180℃,车速为55米每分钟;
步骤D、起绒面料染色:在染色设备中加入所需要的染料,在起绒面料染色前,染色设备先运行5min使得染料均匀,再按照1℃/min的速率升温至50℃并保持15min,再按1℃/min的速率升温至110℃,并保持10min,再按照1℃/min的速率升温至130℃,并保持50min,再按照1.2℃/min的速率降温至100,再按照1.5℃/min速度降温至52℃,出染缸后在160℃和35米/分钟的条件下进行烘干;
步骤E、柔软处理:将步骤D得到的染色后的面料在柔软剂浓度为3%、抗静电剂浓度为1%的溶液中浸轧后并烘干;
步骤F、磨毛定型:对步骤E所得到的面料进行磨毛处理,在165℃和40米车速下烘干定型。
作为上述方案的进一步说明,步骤A中,所制得的白坯布的平方米重量为400-450克每平方米。
作为上述方案的进一步说明,步骤A中,白坯布的织造工艺中,采用两个经轴为底纱经轴和绒纱经轴,均采用8个盘头和满穿的穿纱工艺,绒纱经轴均分为两幅,底纱经轴和绒纱经轴的送经量分别为1080mm/R和2040mm/R。
本发明的有益效果是:本发明所涉及的一种环保经编麂皮绒面料生产工艺,使用了75D/488F的DTY作为绒纱,使用白坯布在经过拉毛、定型、染色、剪毛和定型后,能够形成麂皮绒的效果。在本发明中并没有使用碱对白坯布进行处理来形成麂皮绒效果,避免了在污水处理中碱的影响,既减少了生产成本,还避免了碱处理所带来的影响。
具体实施方式
下面结合具体实施例对本发明进一步说明。
实施例
本实施例所涉及的一种环保经编麂皮绒面料生产工艺,依次包括如下步骤:白坯布的织造、白坯布起毛、起毛面料定型、起毛面料染色、柔软处理、磨毛定型、打卷包装。
本实施例中白坯布的织造中底纱所使用的原料为54D/24F的FDY,绒纱所使用的原料为75D/488F的DTY,白坯布的纬密为26.5针每厘米。所制得的白坯布的平方米重量为400-450克每平方米,本实施例中为420克。
白坯布的织造工艺中,采用两个经轴,分别为底纱经轴和绒纱经轴,均采用8个盘头和满穿的穿纱工艺,绒纱经轴均分为两幅,底纱经轴和绒纱经轴的送经量分别为1080mm/R和2040mm/R,底纱经轴所对应梳栉的垫纱为10/12",绒纱经轴所对应的梳栉的垫纱为10/34"。
在白坯布进行起毛处理。使用3组起毛机,共12辊对定型后的白坯布进行起毛处理,车速为25米,得到起毛面料。
对起毛后的面料进行定型,定型温度为180℃,车速为55米每分钟。
对定型后的起毛面料进行染色。室温下在染色设备中加入所需要的染料,本实施例中所使用的染料为蓝色。并在起绒面料染色前,染色设备先运行5min使得染料均匀。再按照1℃/min的速率升温至50℃并保持15min,再按1℃/min的速率升温至110℃,并保持10min,再按照1℃/min的速率升温至130℃,并保持50min,再按照1.2℃/min的速率降温至100,再按照1.5℃/min速度降温至52℃,出染缸后在160℃和35米/分钟的条件下进行烘干。
对染色后的面料进行柔软处理,是将染色后的面料处理溶液中浸轧,处理溶液中柔软剂浓度为3%、抗静电剂浓度为1%,浸轧后的面料烘干。
对上述步骤所得到的面料进行磨毛后再在165℃和40米车速下烘干定型定型。用砂磨辊(或带)将织物表面磨出一层短而密的绒毛的工艺过程称为磨绒整理,又称磨毛整理。磨毛织物具有厚实、柔软而温暖等特性。
最后将定型后的面料打卷和包装、入库。
Claims (3)
1.一种环保经编麂皮绒面料生产工艺,其特征在于,依次包括如下步骤:
步骤A、白坯布的织造:底纱所使用的原料为54D/24F的FDY,绒纱所使用的原料为75D/488F的DTY,白坯布的纬密为26.5针每厘米;
步骤B、白坯布起毛:采用3组12辊将白坯布进行起毛处理,车速为25米;
步骤C、起毛面料定型:定型温度为180℃,车速为55米每分钟;
步骤D、起毛面料染色:在染色设备中加入所需要的染料,在起绒面料染色前,染色设备先运行5min使得染料均匀,再按照1℃/min的速率升温至50℃并保持15min,再按1℃/min的速率升温至110℃,并保持10min,再按照1℃/min的速率升温至130℃,并保持50min,再按照1.2℃/min的速率降温至100,再按照1.5℃/min速度降温至52℃,出染缸后在160℃和35米/分钟的条件下进行烘干;
步骤E、柔软处理:将步骤D得到的染色后的面料在柔软剂浓度为3%、抗静电剂浓度为1%的溶液中浸轧后并烘干;
步骤F、磨毛定型:对步骤E所得到的面料进行磨毛处理,在165℃和40米车速下烘干定型。
2.如权利要求1所述的环保经编麂皮绒面料生产工艺,其特征在于,步骤A中,所制得的白坯布的平方米重量为400-450克每平方米。
3.如权利要求1所述的环保经编麂皮绒面料生产工艺,其特征在于,步骤A中,白坯布的织造工艺中,采用两个经轴为底纱经轴和绒纱经轴,均采用8个盘头和满穿的穿纱工艺,绒纱经轴均分为两幅,底纱经轴和绒纱经轴的送经量分别为1080mm/R和2040mm/R。