AU427391B2 - The recovery of lead and silver from solution as sulphides - Google Patents
The recovery of lead and silver from solution as sulphidesInfo
- Publication number
- AU427391B2 AU427391B2 AU35477/71A AU3547771A AU427391B2 AU 427391 B2 AU427391 B2 AU 427391B2 AU 35477/71 A AU35477/71 A AU 35477/71A AU 3547771 A AU3547771 A AU 3547771A AU 427391 B2 AU427391 B2 AU 427391B2
- Authority
- AU
- Australia
- Prior art keywords
- solution
- lead
- accordance
- sulphide
- treated
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired
Description
(1t) 427, 4 391 COMMONWEALTH OF AUSTRALIA
PATENT SPECIFICATION (21)35 47 7/71 Class (52) 08.4; 08.1.
Int. Cf. (51) C01g; C01b.
Application Number (21) 35,477/71. Lodged (22) 8th November, 1971.
Complete Specification entitled (54) THE RECOVERY OF LEA]) AND SILVER FROM SOLUTION AS SULPHIDES.
.Lodged 8th November 1971. Accepted 23rd August, 1972. Published 14th September, 1972.
Convention Priority (30) Nil.
Applicant (71) ELECTROLYTIC ZINC COMPANY OF AUSTRALASIA LIMITED and COMMONWEALTH SCIENTIFIC AND INDUSTRIAL RESEARCH ORGANIZATION.
Actual Inventor (72) THOMAS ROBERT SOCTT.
Related Art (56) 25,442/25 08.4; 14.2. 12,552/28 07.6; 08.4. 132,931(7483/46) 83. 1; 08. 1.
The following statement is a full description of this invention, including the best method of performing it known to us I96SI,71-L W. G. Mu-ay, Go-1-1~~n P-1-1t1.C-n ,la
X426-87-ND-21P. C.
47 7/71 This invention relates to.a process for the
recovery of lead and silver values from solution .as
sulphides jn a form easily separable by physical methods,
e.g. filtration.
For the purposes of the present specification and
the appended claims, "sulphur compounds" are defined as
hydrogen sulphide,
monosulphides, hydrosulphides and polysulphides,
and
mixtures of such compounds the said compounds being produced by the reaction of hydrogen sulphide with aqueous alkalis,
the reaction of monosulphide solutions with elemental sulphur,
the reaction of elemental sulphur and aqueous alkalis at elevated temperature, or
the reaction of amine solutions at elevated temperature with elemental sulphur. In-this specification and in the appended claims
the following abbreviations are used:
AAS ammoniacal ammonium sulphate T/Pb total lead
T/NH 3 total ammonia
T/SO 4 total sulphate
g/1 grams per litre
2 427 3 91
477 71 T/S total sulphide 2- S sulphide ion
gsfm gallons per square foot per minute S/S sulphide expressed as sulphur
SO4 /S sulphate expressed as sulphur
S /S elemental sulphur expressed as sulphur
XRD X-ray diffraction
Because of the preponderance of suphide ores of non-ferrous metals, industrial production processes for
non-ferrous metals are presently mostly equipped and
directed to the treatment of metal sulphides. Hence, when metal values are recovered, from solutions, during
hydrometallurgical processing, it is frequently an
advantage that the metals be recovered in the form of sulphides rather than as other metal compounds.
Hydrogen sulphide, ammonium monosulphide and
ammonium polysulphides are frequently used in analytical work for the precipitation of sulphides, but the procedures employed result in precipitates which are
difficult to filter or which must be boiled to allow
reasonable:separation. Poor filtration and the need
to boil the solutions'are of little consquence in small
scale analytical work.but on a production scale such
procedures are economically unfeasible. A recent classification of the filtration
characteristics of slurries by Flood, Porter and Rennie
(Chemical Engineering, June 20th, 1966)V is as follows:
S3- 4 73 91
3,.47 17" Filtration rate gsfm Fast filtering Medium filtering 0.2 to Slow filtering 0.01 to 0.2
Slurries of slow filtering properties in the above classification would be considered unacceptable commercil
ally. For the purppses of the present specification and the
appended claims, "readily filterable" materials are defined
as these having fast filtering and medium filtering
properties as given by the corrected classification of Flood, Porter and Rennie.
Lead and precious metals may be extracted from process residues such as electrolytic zinc plant residues and residues from the acid oxidative treatment of mixed lead- zinc concentrates, by a number of previously described
processes, e.g. leaching with aqueous solutions of chlorines,
amines, or AAS. However, the recovery of saleable or readily treatable products from such solution can be difficult.
Brine solutions may be electrolyzed to produce
metallic lead or treated with a neutralizing agent to
precipitate a basic chloride.
Amine solutions may be electrolyzed or treated with carbon dioxide to precipitate basic lead carbonate.
Lead may be recovered from AAs solutions in a variety of ways, for example:-
by heating to distil off ammonia (see Australian Patent 293,939) and to precipitate monobasic lead sulphate or lead aamonium sulphate 4 4 7 3 91
-3 5, 477/71
by electrolysis to produce lead and lead
dioxide (see Australian Patent 407231)
by warming supersaturated solutions (see. A ustralian Patent 407999) to precipitate
monobasic lead sulphate or lead ammonium
sulphate. The method selected for recovering lead from
solution depends upon the overall requirements of a
particular plant and market. In some circumstances
the above methods may not be suitable and a lead sulphide
product would be preferred.
It has now been unexpectedly found that lead'may be
precipitated from leach liquors (such as are produced by leaching lead-bearing materials with aqueous solutions
of brines, amines or AAS) by the use of sulphur or
sulphur compounds to produce lead sulphide in a readily filterable form. It is also found that precious metal
values such as silver and gold are co-precipitated with
the lead sulphide and are thus available for recovery. The lead sulphide produced is readily amenable to
treatmet in the many existing plants designed for the
treatment of sulphidic materials.
According to the present invention, therefore, a
process for recovery of lead and/or silver values, as
readily filterable sulphides, from solutions containing
the metal values, includes the step of treating the said
solution with sulphur or sulphur compounds, as hereinbefore
4 27 3 1
47 7 71
defined.
The solution from which the lead and/or silver values are recovered may be an aqueous AAS solution.
The sulphides recovered preferably have a filtration rate in excess of 0.2 gsfm. According to one embodiment of the present invention, a solution containing lead and/or silver values is treated.
with a stoichiometric excess of hydrogen sulphide gas, for
a period not less than 1 hour and a temperature in the
range 200 to 50 C to precipitate metals as sulphides in a readily filterable form.
According to another embodiment of the present invention a solution containing lead and/or silver values
is treated with ammonium monosulphide solution in
stoichiometric excess at a temperature in the range of 200
to 70°C to precipitate metal sulphides in a readily
filterable form.
According to another embodiment of the present invention a solution containing lead and/or silver values
is treated with an alkali metal monosulphide solution in
stoichiometric excess at a temperature in the range 200 to
C to precipitate metal sulphides in a readily filter- able form.
According to another embodiment of the present invention a solution containing lead and/or silver values
is treated with a polysulphide solution in amounts
sufficient to provide a stoichiometric excess of sulphide
6- 4273 91
47 7 71
ions at a temperature in the range of 200 to 70 C to
precipitate metal sulphides in a readily filterable form. Polysulphide solutions may be prepared in a variety
of ways, but the preferred procedures are .as follows:- reaction of a solution of sodium, potassium
or ammonium monosulphide .with elemental sulphur
or a source of elemental sulphur at a 0 temperature in the range of 200 to 200 C,
reaction of a solution of sodium, potassium,
ammonium or amine hydroxide with elemental
sulphur or a source of elemental sulphur at a temperature in excess of 70 C,
reaction between gaseous hydrogen sulphide and aqueous ammonia in the presence of sulphur o6 a source of elemental sulphur.
According to another embodiment of the present
invention a solution containing Pb and/or Ag values is treated with greater than twice stoichiometric excess of elemental sulphur at temperatures in the range of 1200 to
200 C and times in the range of 0.25 to 5 hours to precipitate metal sulphides in a readily filterable form. Preferably the precipitation of lead sulphide should
be carried out in such vessels and in such a manner as to
minimise the loss by volatilization of the reactants. The treatment may be carried out in one or more
stages as is convenient to the overall .processing
requirements. Such stages may be operated in either a 7 427391
.3 47 7 71 continuous or batch manner.
It is possible and may be desirable under Certain
circumstances to carry out the leaching and precipitation
operations in a single stage. Thus it has been shown that
pure lead compounds such as lead sulphate and lead
ammonium sulphate may be treated with elemental sulphur
and an aqueous solution of sodium, potassium, ammonium or
amine hydroxide at elevated temperatures to obtain a coarse, crystalline lead sulphide. Similarly, residues produced by the acid oxidation of mixed lead-zinc
sulphide concentrates and which contain elemental sulphur,
may be treated with aqueous ammonia at elevated tempera-.
tures to obtain a solid product containing substantially
all the lead as lead sulphide. The lead sulphide may be
separated from other components of the residue by methods such as screening or froth flotation.
The sulphur or sulphur compounds used as the
precipitant may be added to the metal-bearing solution
in any convenient way until a stoichiometric excess has
been added to the solution. The lead and/or silver present in the solution will be precipitated as sulphides
by such treatment and free sulphide ions will be present.
If the presence of such free sulphide ions is undesirable,
as may be the case in cyclic operations, the excess
sulphide may be removed by the addition of a suitable
small amount of untreated metal-bearing solution
immediately prior to filtration. Such a procedure does -8 427391
.3 4- 7 /71 not affect the filtration properties of the lead sulphide
precipitate since the greater part of the lead is precipitated in the presence of an excess of sulphide. Alternatively the solution containing excess sulphide may
be treated with activated carbon either before or after filtration to remove the precipitated metal sulphide.
Impurities such as zinc and copper which may have been
dissolved during the leaching of the material containing
lead sulphate will also be precipitated by the treatment
used to precipitate lead and silver sulphides.
When polysulphide solutions are used as precipitants
of lead sulphide, some elemental sulphur is simultaneously
precipitated. Such precipitated sulphur may be conveniently recovered from the precipitate and the
product simultaneously up-graded by extraction of the precipitate with ammonium monosulphide solutions, or other convenient solvent for sulphur.
The solutions produced by reaction of elemental
sulphur and aqueous alkalis contain some alkali thiosulphate
which under some circumstances will cause the precipitation of a small amount of lead thiosulphate, as well as lead
sulphide- nd elemental sulphur. Such lead thiosulphate may be left with the lead sulphide since on heating to
relatively low temperatures it decomposes to a mixture
of lead sulphide and lead sulphate; the small proportion
of lead sulphate in the sulphide precipitate would not
interfere with subsequent processing. If it is desirable 9- 4 7391
3.477/71 to avoid any down-grading of the sulphide precipitate,
lead thiosulphate may be removed by extraction with concentrated thiosulphate solutions in which soluble
lead thiosulphate complexes are formed.
When elemental sulphur is used to precipitate lead from AAS or similar solutions by treatment at elevated temperatures, the reactions.are conveniently
carried out in-a pressure vessel to minimise the loss of
solvent. During such reaction portion of the elemental sulphur added is converted to thiosulphate. Some.of this thiosulphate may react and yield lead thiosulphate which
may be conveniently dealt with as described above.
The sulphur required for the production of polysulphide solutions, either by reaction with monosulphide solution or aqueous alkali, may be either
substantially pure elemental sulphur or elemental sulphur
present in ores or process residues.
EXAMPLE 1 Use of hydrogen sulphide
A series of tests was conducted in which a lead- bearing AAS solution (T/Pb 44.6 g/l, T/NH 3 190 g/l, T/SO 4 270 g/1) was treated with hydrogen sulphide gas at 20 C. The time-during which the hydrogen sulphide was added was varied and the principal results obtained are
given in Ta.ble 1.
10 427391
47 7/71 TABLE 1
Test Time of Pulp Filtrate No. gassing filtration Pb content Product (hours) rate (gsfm) (g/l)
1 0.5 <0.01 N.D. PbS 2 1.0 0.24 <0.1 3 1.75 (a) 0.40 5.0 4 1 12(b) 0.51 1
Reduced gas flow rate used.
Gassing for 1 hour followed by 12 hours standing. A similar test conducted at 50°C for 0'.25 hours gave an unfilterable (<0.01 gal./sq.ft./min.) pulp
containing both lead sulphide and lead sulphate.
It is preferred to use a precipitation time of greater than 1 hour and a temperature in the range 200 to
EXAMPLE 2 Use of ammonium monosulphide
A series of tests was conducted in which lead-bearing AAS solutions (T/Pb 56 g/1, T/NH 3 170 g/l, T/SO 4 300 g/1) were treated with various amounts of commercial ammonium monosulphide solution (16% by weight) at various temperatures. The principal results are summarised by Table 2 below:-
11 4273 9
171. I.
TABLE 2 Test Temp. Moles of Slurry Product No. C monosulphide/ filtration PbS %PbSO mole of Pb rate PbS %PbSO 4 (gsfm)
20 0.69 0.017 74.2 20.2 6 70 1.05 0.36 83.6 13.4 7 40 1.05 0.24 89.1 8.7 8 20 1.01 0.12 80.0 12.1 9 50 1.01 0.27 69.5 27.4
It is- preferred to carry out the precipitation of the lead using an excess of sulphide to achieve
commercially acceptable filtration rates. Higher temperatures lead to increased volatilization of ammonia.
The preferred temperature is in the range 200 to
EXAMPLE 3 Use of ammonium polysulphide solution prepared from
sulphur and ammonium monosulphide.
Ammonium polysulphide solutions were prepared by
agitating a process residue containing elemental sulphur
with ammonium monosulphide solution (16% by weight) at room
temperature. The solutions so prepared were used to precipitate lead sulphide from lead-bearing AAS solutions
and the results obtained are summarised in Table 3.
When aich polysulphide solutions are used some
elemental sulphur is simultaneously precipitated and a
subsequent wash of the solid product with ammonium 12 4 2 3 91
47 7/71
rmonosulphide would be desirable. Such a wash would also lessen the content of lead sulphate of the final product.
13 4273 1
-4 7 0 I~n d N v C
o cnT 0 O'I 4-I C dP N 0 *Ir*a V) 0 0 m M- Cl) ON En04 A~ H IN >4 A4
LO H dP' H CO
r-I co0 ININ. 0j -1 M- 0000 C4
P4
(d0 N .,104 0C4-40 *iO N N E-I -4 1 N- 4J.)
dP43 0N a %DO 00 ItO 0 N-
04) .0 9 HDC%L
U)0) It) 4.1 N -4 43) H N I
0 a. 0o H u a) 04H H H
E-4 o 0 it)n I eq -Cr D %q
$04
0.) 0 Ci) IN 00 0* r-4 "I 0) o 0 0- En l 0* 0 Ci) C14 H- %0 C') .0 w -0 UtC to 04 II
H N C)) 100 o 00 m' 0> :1 0- .0 H .0 0
4 JH 0 0~0 N -4 4 N Ij 0 E-I U) C) 014ZnI
14 ~27 3 OIL
3. 47 7/71 EXAMPLE 4 Use of polysulphide solutions prepared from sulphur and aqueous ammonia
Ammonia and sulphur-bearing process residues were reacted together at a temperature of 125°C to produce solutions containing ammonium polysulphide and ammonium thiosulphate. The total sulphur contentof such solutions was determined by the loss in sulphur content of the residues used for their preparation.
Ammonium polysulphide solutions prepared by this procedure were reacted with lead-bearing AAS solutions under various conditions to precipitate lead sulphide. The results of such tests are summarised in Table 4.
15 427 391
35,4 7 7/71
En ciN C'J (N C'j 0
0 -r (N 00 wl H4 0 %D 0 0 0; In N 0; (N CN 4) 4., Ln LA c,
V La 01 L LA i%Q c i o tni 'a 01 01 1 41. V CO 0. 0. H (N H; 0; 0; 4 ta 4J LA wD LA IT 0. 01 H V% -d 01 4.) -4 .0 t C. aL L a~ C U H 01 04-i 0. "-4 01 p4 444N r nI 01 >i V H -4 .La V 00 0 0 0 0 04-4 H .La
.0 01 01 9 -4 rH4) -H N A A 0(NH0 11 04 01N C -4 01 .La 41 4 01 0. H
La 01 -4 4J 1I 01 0 4)LO 0 0 0 0 W 4 10 0 La 01~ 0. 01 0 LA LA 0N Co C 40
.La 0. ~'i H H La 0. 4 (dH .4 H 01 0 04 .I4.L 01 01 01 U 4. 4.4 r- 'r N k 1 V La 0. 0 :3 4-4- -4 H 01 01 E-1 WH' U La V 4 La 'a 0 54 :i 01 a )HD .La 4.) H Oj 0 0 C a 0 0 0 0.01 OH N LA LA LA LND H .La 1.4 0. 01 01 4 -4 04 tl. N CL CLa LA 4 C4 0'i 0 .La E4 4J
'4 aLa -T o 0, o Co H Z N N H
4 j
47 7 17
Use of amine solutions
Solutions of lead sulphate dissolved in diethylene
triamine were boiled for one-hour with elemental sulphur.
Substantially all the lead was precipitated as lead
sulphide which was removed from the resulting pulp by filtration at a filtration rate of greater than 0.1 gsfm.
EXAMPLE 6
Use of elemental sulphur
In a series of tests lead-bearing AAS solutions were
treated with elemental sulphur in an autoclave at various
temperatures. The principal results obtained are given in Table
Autoclave conditions Moles of AAS Product elemental liquor Compo- Run Tmp.Press. Time Sulphur sulphur/ Vol. Pb nents P (by XRD) N. C (psig) (hr) addn Pb of mole (m/s
110 70 5 5.6 2.04 400 44.6 61 PbS+LAS+ S° (a) 21 110 80 6.5 6.0 1.97 400 41.4 72 PbS+LAS+ S° (a)
22 150 120 3.5 18.0 6.80 400 42.6 1oo PbS+S 23 200 400 4.5 7.0 2.25 375 53.8 yoo PbS
LAS PbSO 4 .(NH 4 2 SO 4
17 42 3 91.
3. 47 7,71 Analysis of the solid product from test 23 indicated the
following composition
PbS 98.8%
PbSO 0.6% 4
PbSO4(NH4 2 SO4 0.25% S° 0.3%
EXAMPLE 7
Precipitation of lead from amine solutions
A solution containing 50 g/l Pb and of pH 10.8 was prepared from lead sulphate, ethylene diamine (approx.
21% by weight) and water. This solution was treated at room temperature for 15 minutes with a 16% ammonium
monosulphide solution to give a molar ratio .of sulphide to
lead in the mixtur.e of 0.31. A precipitate was formed which was shown to contain lead sulphide and tribasic lead sulphate
and which filtered at a relative slow rate of 0.19 gsfm. After removal of the precipitate by filtration the
remaining solution, which still contained lead, was treated
with further amounts of ammonium sulphide to give: a molar
ratio of sulphide to lead of 1.24. A precipitate was formed and was removed by filtration. The filtration rate observed was 0.69 gsfm and the product was shown to be substantially
pure lead sulphide.
18 4 -7 3 9.1
3 5 4 777 EXAMPLE 8
Precipitation of silver
A solution was prepared of the following
composition:-
Pb 47.4 g/l
Ag 0.104 g/l
T/SO4 284 g/l
T/NH3 179 g/1 by leaching a silver-bearing lead sulphate with AAS solution. A solution of ammonium monosulphide contain- ing 53.5 g/l S/S was also prepared.
400 mis of solution containing 19 g of lead and 57.5 mis of solution were mixed at 60°C for 25 minutes. The molar ratio of sulphide to lead in the mixture was 1.05 and thus the excess sulphide present was equivalent to 0.93 g of lead. A further 100 mis of solution containing 4.74 g of lead was added and the mixture filtered. Hence the greater part of the lead in the sulphide precipitate was precipitated with an excess of sulphide present. The filtration rate observed was 0.41 gsfm. 86.0% of the lead and >99.9% of the silver originally present in the solution' were recovered in the sulphide precipitate.
The solution after-filtration was shown to be free of sulphide ions and hence would be suitable for re-use in leaching further material.
19
47 7/71 EXAMPLE 9
Precipitation of lead from brine solutions
A solution which contained 16.5 g/l lead was
prepared by leaching lead sulphate with a concentrated
sodium chloride brine solution (approx. 260 g/1). Solution was treated with an excess of 16% 0 ammonium monosulphide at pH 7.0 for 30 minutes at 25 C.
The resulting pulp was filtered at a rate of 0.55 gsfm and the solids were shown to be lead sulphide.
20
Claims (1)
- 47 7 7 The claims defining the invention are as follows:-1. A process for the recovery of lead and/or silvervalues as sulphides in readily filterable form, as herein-before defined, from solutions containing the metal valueswhich includes the step of treating the said solution witha stoichiometric excess of sulphur or sulphur compoundsas hereinbefore defined.2. A process in accordance with claim 1 in which thesolution from which the lead and/or silver values are recoveredis an aqueous ammonical ammonium sulphate solution.3. A process in accordance with claim 1 or claim 2 inwhich the sulphides have a filtration rate in excess of 5 gsfm.A. A process in accordance with any one of claims 1 to 3in which the solution containing lead and/or silver values istreated with a stoichiometric excess of hydrogen sulphidegas for a period not less than one hour and at atemperature in the range 20 0 C to 500C.A process in accordance with any one of claims 1to 3 in which the solution containing lead and/or silvervalues is treated with ammonium monosulphide solution instoichiometric excess at a temperature in the range 200Cto 700C.6. A process in accordance with any one of claims 1to 3 in which the solution containing lead and/orsilver values is treated with an alkali metal monosulphidesolution in stoichiometric excess at a temperature inthe range 20°C to 70 0 C.S 21 4273913 .4 7 7,71 7. A process in accordance with any one of claims 1 to 3 in which the solution containing lead and/or silver values is treated with a polysulphide solution in sufficient amounts to provide a stoichiometric excess of sulphide ions at'atemperature in the range 200 C to 8. A process in accordance with claim 7 in which the polysulphide solution is prepared by reaction of elementalsulphur or .a source of elemental sulphur and sodium, potassium or ammonium monosulphide solution at atemperature in the range 20°C to 200 0 C., 9. A process in accordance with claim 7 in which the polysulphide solution is prepared by reaction of elementalsulphur or a source of elemental sulphur and sodium,potassium, ammonium or organic amine hydroxide solution ata temperature in excess of 700C. A process in-accordance with any one of.claims 1 to 3 in which the solution containing lead and/or silver valuesis treated with greater than twice the stoiddcmnetric excessof elemental sulphur ap temperatures in- the range of 120 0 C 4 o to 200 0 C4 "4 iPV Lk11. A process in accordance with claim 1 in which asodium ch-loride or calcium chloride solution containing lead and/or silver values is treated with a solution of sodium,potassium or ammonium sulphide in stoichiometric excess at a r0°C. temperature in the range of 20 C to/.4e.22 427391477/71 12. A process in accordance with claim 1 in which an aqueous solution of an organic amine containing lead and/orsilver values is treated with a solution of ammonium .sulphide in stoichiometric excess at a temperature in therange of 20°C to 700 C.DATED this 5th day of NOVEMBER, 1971. ELECTROLYTIC ZINC COMPANY OF AUSTRALASIA LIMITED and COMMONWEALTH SCIENTIFIC AND INDUSTRIAL RESEARCH ORGANIZATION By their Patent Attorneys:CLEMENT HACK CO. Fellows Institute of Patent Attorneys of Australia.23