AU465647B2 - Latexes for cathodic electrocoating - Google Patents

Latexes for cathodic electrocoating

Info

Publication number
AU465647B2
AU465647B2 AU41492/72A AU4149272A AU465647B2 AU 465647 B2 AU465647 B2 AU 465647B2 AU 41492/72 A AU41492/72 A AU 41492/72A AU 4149272 A AU4149272 A AU 4149272A AU 465647 B2 AU465647 B2 AU 465647B2
Authority
AU
Australia
Prior art keywords
aqueous dispersion
sulfonium salt
water
sulfonium
percent
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
AU41492/72A
Other versions
AU4149272A (en
Inventor
EARL HENRY WAGENER and RITCHIE ANTONE WESSLING DALE SABIN GREBS
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dow Chemical Co
Original Assignee
Dow Chemical Co
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dow Chemical Co filed Critical Dow Chemical Co
Publication of AU4149272A publication Critical patent/AU4149272A/en
Application granted granted Critical
Publication of AU465647B2 publication Critical patent/AU465647B2/en
Expired legal-status Critical Current

Description

41,492/72 The present invention relates to cationically
stabilized latexes which are suitable to form coatings
especially by electrodeposition, and to a process for
preparation of such latexes.
In the commonly used processes of electrodepo-
sition, latex compositions are employed which are stabili-
zed with anionic emulsifiers and such compositions are de-
posited at the anode. Certain electrodeposition systems
which use cationic nitrogen-containing surfactants have
been described, such as in United States patent 3,454,482
and 3,455,806, both issued to Spoor et al., July 8, 1969
and July 15, 1969.
In the previously published descriptions of com-
positions which have been used for electrodeposition of
coatings or have been recommended for such use, there has
been no disclosure that the emulsifiers are electrically
reducible under the usual conditions for electrodeposition
or are thermally degradable under conditions which would not
harm the coating.
In accordance with the present invention, aqueous
dispersions of organic film-forming polymers, suitable for
cationic electrodeposition as coatings, are prepared under
usual emulsion polymerization conditions from polymerizable,
ethylenically unsaturated monomers, which when homopolymeri-
zed or copolymerized with each other form water-insoluble
polymers, and together therewith from about 0.5 part to
about 10 parts preferably from about 2 parts to about
parts per 100 parts of the total monomer composition of a
polymerizable sulfonium salt, optionally in the presence of
small amounts such as less than about 5 parts, on the same
465,647
41,492 72 basis, of conventional sulfonium surfactants.
The resulting aqueous dispersions provide electrodeposi- coatings, especially by means of cationic materials tion, that release smaller amounts of volatile which utilize when the coatings are heated than dispersions type to pro- only conventional surfactants of the same the means of vide dispersion stability and to provide
transport in an electrodeposition system. require The aqueous dispersions of the invention unsaturated, copolymers of a polymerizable, ethylenically
water-soluble sulfonium salt. An illustrative formula for
such salts is 2
R' nA- R3 n
aliphatic, wherein R' is an n-valent organic radical, ethylenic un- aromatic or alicyclic, having polymerizable 3 saturation, R 2 and R individually are alkyl, monohydroxy-
A- is a water- substituted alkyl, cycloalkyl, or aralkyl, ordinarily 1 or 2. soluble anion and n is an integer, but R' and R 2 and R 3 primarily constitute hydrocarbon chains such as oxygen, the chains can be interrupted with linkages or amide linkage. sulfur and nitrogen or by a keto, ester 2 3 R and R often is less The sum of the carbon atoms in in the salt molecule. than about 16 for each sulfonium group
The specific identity of the counterion A- is not
critical. The counterion should not coagulate the dispersion state. nor react with the sulfonium ion in the dispersed
Representative, but not limiting, examples are chloride, bicarbonate acetate, nitrate, propionate, hydrogen sulfate,
465,647
41,492/72 and hydrogen phosphate. Certain specific monomeric sulfonium salts are those of Formula I wherein R2 and R3 n and A are as
shown in Table I. It should be recognized that these are illustrative representative operable materials and the listing by no means should be considered as all inclusive.
465, 647
41.492 /72
1- 1- -4
IA c cn, cn c'J cn 6 1
U, C., cn c -n n c. CI 16 C.)
c..J C.) C', C.) C.)
C-,
C.) C.) U II U a 0 C', C." C',
C.) C.) C.) C.)
1; C4J
4 65, 647
4 1.4 92 g
0 0 ,4 0 '-4
c'J
ra ra r-I r-I r-4 v-
0
C4
0
C14 0'4 1.
C, 0 14 C14 00 0. 0, L C'4
CN) c.)
C14 oq C- 0 SU 6 6 ci CN E; C)
0 r4 -4 r4i 4 r4 r4~ '0 r
4 6 5.647
4 1,492/72n
_4 0 0 L
4 C m4
C14
co 0
-4 -4
4 65 647
41.492/72 The aqueous dispersions of this invention con-
tain copolymers of the monomeric sulfonium salts as
described with an essentially hydrophobic, polymeriz-
able ethylenically unsaturated monomeric composition con-
taining one or more polymerizable, ethylenically unsatura-
ted compounds which when homopolymerized or copolymerized
with each other form water-insoluble polymers, hierein
the monomeric sulfonium salts ordinarily are used in an
amount of from about 0.5 part to about 10 parts, preferably
from about 2 parts to about 5 parts, for each 100 parts by
weight of the total monomeric composition, but in any
event are not used in sufficient quantity to make the poly-
mer water-soluble.
Neutral,electrically non-conductive, polymeriz-
able,ethylenically unsaturated compounds are represented
by, but not restricted to, non-ionic monomers such as the
alkenyl aromatic compounds, the styrene compounds;
the derivatives of a-methylene monocarboxylic acids such
as the acrylic esters, acrylic nitriles and methacrylic
esters; derivatives of a,P-ethylenically unsaturated dicar-
boxylic acids such as maleic esters; unsaturated alcohol
esters; conjugated dienes; unsaturated ketones; unsaturated
ethers; and other polymerizable vinylidene compounds such
as vinyl chloride and vinylidene fluoride. Specific examp-
les of such ethylenically unsaturated compounds are styrene,
a-methylstyrene, ar-methylstyrene, ar-ethylstyrene, a-ar-di-
methylstyrene, ar,ar-dimethylstyrene, ar,ar-diethylstyrene,
t-butylstyrene, vinylnaphthalene, hydroxystyrene, methoxy-
styrene, cyanostyrene, acetylstyrene, monochlorostyrene, di-
chlorostyrene, and other halostyrenes, methyl methacrylate,
a 465647
41.492/72 ethyl acrylate, butyl acrylate, hexyl acrylate, 2-ethyl-
hexyl acrylate, lauryl methacrylate, phenyl acrylate,
2-hydroxybutyl acrylate, 2-hydroxybutyl methacrylate,
4-hydroxybutyl acrylate, and 4-hydroxybutyl methacrylate;
acrylonitrile, methacrylonitrile, acryloanilide, ethyl
a-chloroacrylate, ethyl maleate, vinyl acetate, vinyl pro-
pionate, vinyl chloride, vinyl bromide, vinylidene chlo-
ride, vinylidene fluoride, vinyl methyl ketone, methyl iso-
propenyl ketone, vinyl ethyl ether, 1,3-butadiene, and
isoprene.
Such non-ionic monomers form water-insoluble ho-
mopolymers or water-insoluble copolymers when more than one
of the group is used. Ibwever, there may be used as copoly-
merized constituents with the above kinds of monomers other
non-ionic monomers which as homopolymers would be water-
-soluble. The hydrophilic, water-soluble, non-ionic mono-
mers are represented by hydroxyethyl acrylate, hydroxyethyl
methacrylate, acrylamide, methacrylamide, N-methylol acryl-
amide, N-methylol methacrylamide and other modified acryl-
amides such as diacetone acrylamide, and diacetone methacryl-
amide.
Such monomers, or the other more hydrophilic mo-
nomers described infra, are not used in sufficiently large
proportions as to make the copolymer water-soluble or sig-
nificantly electrically conductive. The proportion of such
somewhat hydrophilic, water-soluble, non-ionic monomers which
may be copolymerized constituents of the polymers operable
in the practice of this invention ordinarily ranges from 0
to about 30 percent or more based on the total weight of the
copolymer.
A65,647
41,492/72 as Other more hydrophilic monomers may be used proportions, such constituents of the copolymers in smaller
less than about 4 percent by weight. These hydrophilic as, esters of a,P-eth- monomers are represented by aminoalcohol of such lenically unsaturated carboxylic acids, especially by acry- acids having from 3 to 5 carbon atoms, illustrated fumaric acid, and lic acid, methacrylic acid, maleic acid,
itaconic acid; for example, 2-aminoethyl methacrylate hydro- 2-aminopropyl chloride, 2-aminoethyl acrylate hydrochloride,
acrylate hydrochloride, 2-aminopropyl methacrylate hydrcchlo-
ride, 3-aminopropyl methacrylate hydrochloride and other States Patent No. amino alcohol esters as described in United 29, 1963. 3,108,979, issued to LeFevre et al, October hy- In the specification, by the term "essentially monomer drophobic, polymerizable, ethylenically unsaturated monomers accor- composition" is meant a monomer or mixture of
ding to the foregoing description.
The aqueous dispersions of this invention are
conveniently prepared from the above-described monomers by
free-radical pro- conventional emulsion polymerization using 0.01 percent ducing catalysts usually in an amount from about monomers under to about 3 percent based on the weight of the pressure, and conventional conditions of agitation, time, or contin- temperature, using either a batchwise, incremental
uous type addition of the monomers, water and other constitu-
vessels, or ents to a reaction vessel or to a series of such
by polymerization in a coil reactor. Conventional additives
but usual for latex composition may be included in small
amounts and in a known manner. Such materials include, but
short stopping are not restricted to, chain transfer agents,
41,492 72 agents, buffers, anti-foaming agents, chelating agents,
inorganic salts, plasticizers, tinting materials and bac-
tericides, or other preservatives. Small amounts of non-
-ionic or cationic surfactants may also be employed,*par-
ticularly when using the lower amount of the monomeric sul-
fonium salts. To minimize their effect on subsequent elec-
trodeposition behavior usually there will be used the smal-
lest amount of added surfactants which gives the desired
effect, such as particle size control or a particular de-
gree of dispersion stability. Sometimes these surfactants
are introduced into the polymerization mixtures as a compo-
nent of a preformed seed latex. In a preferred process, to
small amounts of a seed latex are added water, the polymeri-
zable sulfonium salts, the other constituent monomers, the
free-radical producing catalysts and any other ingredients
of the emulsion polymerization recipe in an incremental or
a continuous manner while maintaining agitation of the con-
tents of the polymerization zone under conditions of pres-
sure suitable for the monomeric composition being used and
at a temperature suitable for the particular catalyst sys-
tem and the decomposition temperature of the sulfonium salt
being used, such temperatures usually being between about
0°C. and about 100°C., preferably below about 70°C. It is
often advantageous to keep the rate of monomer addition low
enough so that the monomer addition rate controls the rate
of polymerization.
The catalysts are of the type which produce free-
radicals and conveniently are per-oxygen compounds for exam-
ple, the inorganic persulfate compounds such as sodium per-
sulfate, potassium persulfate and ammonium persulfate;
465,647
4 1,4 92/72 the inorganic peroxides such as hydrogen peroxide; the or-
ganic hydroperoxides such as cumene hydroperoxide and t-
-butyl hydroperoxide; the organic peroxides such as benzoyl
peroxide, acetyl peroxide, lauroyl peroxide, peracetic acid
and perbenzoic acid sometimes activated by water-soluble
reducing agents such as a ferrous compound, sodium bisul-
fite or hydroxylamine hydrochloride-- and other free-radical
producing materials such as 2,2'-azobisisobutyronitrile.
The aqueous dispersions, the latex composi-
content tions, usually are prepared at a polymer solids
from about 35 percent to about 60 percent, preferably from
about 40 percent to about 50 percent. When the dispersions
are used for an electrodeposition process, they ordinarily con- are diluted with water to give a desired lower solids about tent before use such as from about 2 percent to
percent, preferably from about 5 to about 12 percent.
While the latex products of the invention may be
used for a wide variety of purposes, especially coatings use in of various types, they are particularly desirable for over a electrodeposition processes which can be carried out
wide range of pH to coat materials having an electroconduc-
tive surface such as steel, copper, aluminum, phosphated
steel and conductive polymers. They are also advantageous
for use in other deposition systems where a low ionic con-
tent is desirable such as in electroconductive papers.
The compositions of the invention, when used for
electrodeposition, are advantageous compared with the widely
used anodic systems in that they are deposited at the cath-
since ode rather than the anode and thus in coating metals,
oxidation reactions do not occur at the cathode, no metal
12 465.647
41,492 /72 process to ions are produced in the electrodeposition The compositions cause coagulation and discoloration. prior art compositions also are advantageous compared with electrodeposition proces- used in both anodic and cathodic which provide the ses in that while the anions or cations and cationic sys- means of transport in the known anionic continue to be points tems remain with the polymers and cations of the poly- of moisture sensitivity, the sulfonium invention will decom- merized sulfonium salts of the present during the electrodeposition pose into hydrophobic products the coated material. The and during subsequent heating of compared with aqueous dis- compositions are advantageously sulfonium surfactants persions stabilized with conventional by-products are obtain- in that a lesser quantity of volatile are heated. Further- ed when the electrodeposited coatings weight materi- more, in those instances where low molecular final product are intro- als which are undesirable in the by the preparative duced intentionally or inadvertently them by dialysis, the pro- steps and it is desired to remove dispersion stability ducts of the invention possess greater prepared using only during and after dialysis than products
conventional surfactants. to an electro- In this specification, references
of a latex for cationic deposition test for suitability to a test which is car- electrodeposition processes relate indicated otherwise: ried out as follows unless specifically tested is diluted In procedure A the latex being and 70 grams with water to a solids content of 10 percent, a rectangular poly- of the diluted latex is introduced into 107 mm long, 25.4mm wide and ethylene electrodeposition cell
465,647
41.4 92/72 79 mm. deep containing two graphite anodes of equal size
located at the ends of the long axis. A rectangular test panel of phophated steel, except as otherwise indicated,
102 mm. long, 18 mm. wide, and 1.6 mm. thick is placed in
the latex to a depth of 20.2 mm. halfway between the two
anodes with the flat 102 mm. by 18 mm. plane normal to a
line joining the two anodes and the length dimension ori-
ented vertically. A source of direct current at a poten- tial of 200 volts is connected to the two anodes and the
steel sample which functions as the cathode. At the end of two minutes, the residual current is measured, the
source of current is disconnected, then the coatings are
examined, the coating weight determined and the efficiency,
expressed as weight of coating per coulomb, is determined.
Procedure B is the same as procedure A except that the electrodeposition cell is 50 mm. wide, 114 mm.
long and 140 mm. deep; the steel test panel is 149 mm.
long, 70 mm. wide and 0.63 mm. thick; the test panel is
placed in the cell between the graphite anodes 1.9 mm. from
each, with the length dimension of the panel oriented ver-
tically and sufficient latex is used to cover the test
panel to a depth of from 70 to 72 mm.
The following examples illustrate the present invention. All parts and percentages are calculated by weight unless otherwise expressly indicated.
Example I
Into a polymerization vessel were charged 5 parts of a 30 percent solution of hydrogen peroxide, 0.0039 part of ferric chloride hexahydrate, 100 parts of water, suf- ficient hydrochloric acid to adjust the pH to 2.5, 0.7 part
IA '465,647
41,492 72 of vinylbenzyl dimethyl sulfonium chloride, 24 parts of
styrene, 8 parts of vinylbenzyl chloride and 48 parts of
n-butyl acrylate. The contents of the polymerization
vessel were stirred for 25 hours at 700C.
There was obtained thereby a stable latex at an
acid pH having a solids content of 42.5 percent, and con-
taining vinylbenzyl dimethyl sulfonium chloride in copoly-
merized form.
The latex was tested in the electrodeposition pro-
cess (procedure A) described supra. For five replicate
samples, coatings which were smooth and uniform were de-
posited having an average thickness of 0.4 mil (0.010 mm.)
with an efficiency of 10.4 mg. of coating per coulomb and
the residual current was 3.0 milliampers.
Example II
A monomer solution was prepared from 960 parts of
n-butyl acrylate and 640 parts of styrene with 5.0 parts
of a catalyst, tertiary-butyl hydroperoxide (82.7 percent
active).
In a seed step 25 parts of the monomer solution,
750 parts of distilled water, 10 parts of dodecylbenzyldi-
methyl sulfonium chloride and sufficient acetic acid to
give a pH of 3.5 were introduced into a polymerization ves-
sel and the temperature of the resulting mixture was held
at 30°C., the system was purged with nitrogen, then there
was added in a continuous manner at a rate of 7.67 parts
per hour an aqueous solution of hydroxylamine hydrochloride
at a concentration of 1.8 parts per 100 parts of water
while the contents of the reactor were stirred. The mixture
was observed for the appearance of blue turbidity which in-
46 5,647
41,492 /72 dicated a small particle-sized latex was being formed and the "seed reaction" was then continued for an addi- tional 90 minutes. A monomer stream from the previously prepared monomer mixture was added at the rate of parts per hour for 20 hours. Concurrentlytherewith, an
emulsifier solution at a pH of 3.5 prepared from 25 parts of dodecylbenzyl dimethyl sulfonium chloride, 27.5 parts of vinylbenzyl dimethyl sulfonium chloride and 500 parts of water was added at a rate of 20 parts per hour. The
addition of hydroxylamine hydrochloride solution was con- tinued for about one hour after the addition of the monomer solution and of the emulsifier solution were discontinued. A stable latex product was obtained having an average par- ticle size of 1010 Angstroms, a solids content of 46.3 per- cent, and a pH of 3.1. A portion of the latex product in the electrode- position test (procedure A) provided a coating of 0.050 mg./mm. 2 with a residual current of 3.5 milliamperes and an efficiency of 9.2 mg. per coulomb. Example III Another latex was prepared in the same manner using the same materials in the same proportion as in Exam- ple II except that allyl dimethyl sulfonium chloride was substituted for the vinylbenzyl dimethyl sulfonium chloride. The stable latex product had an average particle size of 2200 Angstroms, a solids content of 44.4 percent, a Ph of and contained allyl dimethyl sulfonium chloride in co- polymerized form. In the electrodeposition test (procedure the
residual current was 0.4 milliampere and a smooth, uniform,
4i 46647
41.492/72 thin coating was applied to the steel sample at a coat- ing weight of 0.013 mg./mm. 2 with an efficiency of 12.1 mg. per coulomb. Example IV Another latex was prepared as described in Example II using the same materials in the same propor- tions and in the same procedural steps except that for the vinylbenzyl dimethyl sulfonium chloride theiewas substitu- ted an equal amount by weight of dimethyl (2-methylene- -3-butenyl) sulfonium chloride. The stable latex product had an average particle size of 975 Angstroms, a solids content of 48.1 percent, a pH of 4.3 and contained the di- methyl (2-methylene-3-butenyl) sulfonium chloride in copo- lymerized form. In the electrodeposition test (procedure A) the residual current was 1.4 milliamperes and a smooth, uni- form, thin coating was applied to the steel sample at a coating weight of 0.014 mg./mm. 2 and an efficiency of 12.5
mg. per coulomb.
Example V
Into a pressure polymerization vessel were
placed 8.75 g. of phosphoric acid, 20 g. of dodecylbenzyl
dimethyl sulfonium chloride, sufficient water to provide
2000 ml. of solution and sufficient ammonium hydroxide to
give a pH of 5. After flushing the vessel three times with
vacuum and nitrogen, 50 g. of styrene and 50 g. of butad-
iene were introduced, then the contents of the polymeriza-
tion vessel were stirred and maintained at a temperature of 0 C. A continuous stream of catalyst solution, which had
been prepared from 32.5 g. of tertiary-butyl hydroperoxide
465, 647
41.492/72 (87.4 percent active) in 500 ml. of water, was started
in a continuous manner at a rate of 10 ml. per hour.
Concurrently therewith a solution which had been prepared
from 14 g. of hydroxylamine hydrochloride in 500 ml. of
water was added continuously at a rate of 10 ml. per hour.
The resulting seed reaction was continued for three hours,
then the main monomer mixture which had been prepared pre-
viously from 1200 g. of styrene, 1500 g. of butadiene and
300 g. of acrylonitrile was introduced as a continuous
stream at the rate of 110 g. per hour for 19.5 hours, and
concurrently therewith an emulsifier stream at the rate of ml. per hour which had been prepared previously from 100
g. of dodecylbenzyl dimethyl sulfonium chloride, 90 g. of
an aqueous solution containing 63.3 percent of vinylbenzyl
dimethyl sulfonium chloride, sufficient water to provide
1000 ml. of solution and sufficient ammonium hydroxide to
give a pH of 5. The addition of the solutions of tertiary-
-butyl hydroperoxide and of hydroxylamine hydrochloride
were continued for about one hour after completion of the
monomer and emulsifier streams. There was obtained there-
by a stable latex containing vinylbenzyl dimethyl sulfonium
chloride in copolymerized form. The latex had a solids con-
tent of 43.2 percent, a particle size of 1230 Angstroms,
a pH of 2.5 and a surface tension of 45 dynes/cm.
A portion of the latex was tested in the electro- deposition process (procedure B) on phosphated steel and uncoated steel. The results, as an average of two samples were as follows:
465.647
41,492/72 Phosphated Uncoated Steel Steel Coating weight, mg/mm 2 0.053 .025 Residual current, milli- 60 100 amperes Efficiency, mg. of coat- 9.6 7.7 ing/coulomb
Example VI
A latex was prepared substantially as describ-
ed in Example II except that 1600 parts of n-butyl acry-
late was used instead of a mixture of styrene and n-butyl
acrylate, the amount of catalyst was 9.5 parts instead of parts; in the monomer portion of the seed step
parts of the monomer were used instead of 25, and in the aqueous portion of the seed step, the amount of water was adjusted to give a total of 1000 parts of aqueous solution,
and the emulsifier stream was added at the rate of 20 parts
per hour of an aqueous solution of 62.5 parts of dodecyl-
benzyl dimethyl sulfonium chloride and 43 parts of an
aqueous solution containing 63.8 percent of vinylbenzyl
dimethyl sulfonium chloride which was diluted with water to a total of 500 parts. There was obtained thereby a very
stable latex containing a copolymer of n-butyl acrylate and vinylbenzyl dimethyl sulfonium chloride and having a solids
content of 43.3 percent,a pH of 2.5, a surface tension of 30.8 dynes per centimeter, and a particle size of 1300
Angstroms.
A portion of the latex product in the electrode-
position test (procedure B) gave a very smooth, uniform
coating on the steel sample with a coating weight of 0.049 mg./mm.2, a residual current of 75. milliamperes and an
n 465,647
41.492/72 efficiency of 12 mg. of coating per coulomb calculated
as an average of duplicate determinations.
Example VII
A latex was prepared substantially as describ-
ed in Example VI except that 1120 parts of n-butyl acry-
late and 480 parts of methyl methacrylate were used in-
stead of 1600 parts of n-butyl acrylate, and the tempera-
ture for the process was 50°C. rather than 300 C. The
product was a stable latex having a particle size of 1280
Angstroms, a solids content of 42.8 percent, a pH of
and a surface tension of 30.8 dynes per centimeter.
A portion of the latex in the electrodeposition
test (procedure B) provided a thin coating on the steel 2 test panel at a coating weight of 0.048 mg./mm. with a
residual current of 75. milliamperes, and with an effic-
iency of 11.4 mg. of coating per coulomb.
465,647

Claims (1)

  1. 41.492/72 THE CLAIMS DEFINING THE INVENTION AE; A3 FOLLOJ3:-
    1. An aqueous dispersion comprising an aqueous
    medium having stably dispersed therein a water-insolublp
    copolymer of a hydrophobic, polymerizable, ethylenicall
    unsaturated monomer composition and from 0.5 percent to
    percent based on the total weight of the copolymerize-
    monomers of a polymerizable, water-soluble, ethylenically
    unsaturated sulfonium salt, wherein the dispersion stability
    is provided at least in part by the copolymerized sulfonium
    salt.
    2. The aqueous dispersion of Claim 1 in which the
    water-soluble sulfonium salt has the formula
    R2 1 nA
    13 R n
    wherein R' is an aliphatic, aromatic or alicyclic organic
    n-valent radical having polymerizable ethylenic unsaturation,
    R 2 and R individually are alkyl, monohydroxy-substituted alkyl, cycloalkyl, or aralkyl, A7 is a water-soluble anion,
    n is 1 or 2, and wherein R 2 and R 3 primarily constitute hydrocarbon chains which can be interrupted by oxygen,
    nitrogen or sulfur or by a keto, ester or amide linkage.
    3. The aqueous dispersion of Claims 1 or 2, in which
    the sulfonium salt is present in an amount of from 2 percent
    to 5 percent based on the total weight of the copolymerized
    monomers.
    4. The aqueous dispersion of Claims 1, 2 or 3, in
    which the sulfonium salt is a vinylbenzyl dialkyl sulfonium
    465,647 salt. 41.492/72 The aqueous dispersion of Claim 4 in which the salt. sulfonium salt is a vinylbenzyl dimethyl sulfonium
    6. The aqueous dispersion of Claims 1, 2 or 3, in
    which the sulfonium salt is an allyl dimethyl sulfonium
    salt.
    7. The aqueous dispersion of Claims 1, 2 or 3, in dimethyl which the sulfonium salt is a 2-methylene-3-butenyl
    sulfonium salt.
    8. The aqueous dispersion of any of Claims 2 to 7
    in which the water-soluble anion is chloride.
    9. The aqueous dispersion of any of Claims 1 to 8
    in which the hydrophobic monomer composition consists of
    one or more neutral, electrically non-conductive, poly-
    merizable, ethylenically unsaturated compounds. The aqueous dispersion of Claim 1 substantially
    as herein described with reference to any one of the Examples.
    DATED .5th September, 1975.
    PHILLIPS ORMONDE AND FITZPATRICK, Attorneys for
    THE DOW CHEMICAL COMPANY.
    465,647-
AU41492/72A 1971-04-30 1972-04-24 Latexes for cathodic electrocoating Expired AU465647B2 (en)