BE712285A - - Google Patents

Info

Publication number
BE712285A
BE712285A BE712285DA BE712285A BE 712285 A BE712285 A BE 712285A BE 712285D A BE712285D A BE 712285DA BE 712285 A BE712285 A BE 712285A
Authority
BE
Belgium
Prior art keywords
sep
group
products
content
alkaline earth
Prior art date
Application number
Other languages
English (en)
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed filed Critical
Publication of BE712285A publication Critical patent/BE712285A/fr

Description


   <Desc/Clms Page number 1> 
 



  "MINERAIS   AGGLOMERAS   ET LEURS   PROCEDES   DE FABRICATION" 
La présente invention concerne des minerais agglomérés, ainsi que des procédés de fabrication de cos   agglomé-   rats, en particulier des minerais de fer agglomérés d'une haute résistance et au moins partiellement auto-réducteurs, ainsi que des   procédés   de fabrication de ces agglomérats. 



   Depuis   longtemps,   on connaît la nécessité de trouver un procédé   satisfaisant   pour agglomérer les minerais de fer et autres minerais, en particulier les minerais   d'oxydes..   Etant donné qye les minerais   agglomérés   de haute pureté des variétés   mésabite   et autres sont épuisés, il a été nécessaire de se tourner vers des concentrais de mine- rais récupérés de dépôts de minerais moins purs, ainsi que vers de fins minerais qui, jusqu'à présent, n'étalant pas considérés   appropriés   pour la fabrication de l'acier.

   Afin de rendre ces minerais appropriés pour les traiter et les 

 <Desc/Clms Page number 2> 

 utiliser dans des fours de fusion d'acier, il a été nécessaire d'agglomérer ces minerais en plus gros morceaux,   A   cet effet, on a habituellement transformé les fins minerait en boulettes ou en briquettes, puis on a soumis les boulettes ou les briquettes à un frittage ou une fusion, pour former les agglomérats solidifiés. Le frittage nécessite des températures extrêmement élevées et il implique d'importants investissements dans l'équipement résistant   à   ces tempéra-   tures.   



   La demanderesse a trouvé un Minerai aggloméré, ainsi qu'un procédé de fabrication de cet agglomérat beaucoup moins coûteux que ces agglomérats frittés, tout en étant au moins partiellement auto-réducteur. 



   Dans la forme de réalisation préférée de la présente invention, on mélange des fines de minerais avec un oxyde ou un hydroxyde d'un métal   alcalino-terreux,   une ma-   tlère   carbonée finement divisée et éventuellement une faible quantité d'un sel d'un acide minéral d'un métal alcalin ou un métal   alcalino-terreux   et/ou une faible quantité   d'un   hydroxyde alcalin avec suffisamment   d'eau-pour   permettre la formation d'agglomérats tels que des boulettes, des   bri--   quettes ou des blocs. On soumet ensuite ces agglomérats   à   une atmosphère d'anhydride carbonique pendant une période suffisante pour transformer une majeure partie de l'hydro- xyde ou de l'oxyde   alcalino-terreux   en carbonate. 



   On a trouvé que, pour   la   mise en oeuvre la plus efficace du procédé de l'invention, la teneur en humidité devait être inférieure à   10%   en poids du mélange total et, de préférence d'environ 5% ou moins. 



   De préférence, la matière carbonée utilisée dans le procédé de l'invention est du charbon finement divisé. 



   La grosseur préférée pour le charbon utilisé se situe dans l'intervalle de 4 mailles et moins et l'on a obtenu de bons 

 <Desc/Clms Page number 3> 

 résultats aux deux extrémités de cet intervalle, ainsi qu'avec des mélanges de charbon de granulométries variables. 



  On a trouvé que des quantités comprises entre environ 5 et   15   en poids de charbon étaient des plus satisfaisantes .pour l'objet de l'invention, encore que, lors de la mise en oeuvre de ce procédé, on ait employé avantageusement de plus grandes quantités allant jusqu'à   25%.   On a trouvé qu'en employant du charbon à   -100   mailles, on pouvait transformer, en boulettes ou en pastilles, un concentrât d'hématite spé- culaire habituelle "telle quelle" sans ajouter de   l'hématite   rebroyée ou sans ajouter un autre fin minerai. Antérieure- ment, il était impossible de former des boulettes ou des pastilles d'hématite spéculaire par les méthodes classiques sans   rebroyer   ou ajouter un autre fin minerai.

   Ce fut là un des problèmes cruciaux des types de pastilles durcis à la chaleur et fabriqués jusqu'à présent ot   c'est   là   égale-   ment un avantage très net résultant de la mise en oeuvre de la présente invention. On a trouvé que l'on pouvait réa- liser cet objet avec les concentrations en charbon comprises dans les intervalles définis ci-dessus, bien qu'il soit préférable d'employer environ 10% de charbon à -100 mailles lorsqu'on forme des boulettes ou des pastilles d'hématite spéculaire. 



   De préférence, la quantité d'hydroxyde ou   d'oxy-   de alcalino-terreux, par exemple la chaux, se situe dans l'intervalle d'environ 5 à   20%   on poids du mélange. 



   Il est préférable d'ajouter une faible quantité (jusqu'à environ   2%)   d'un agent solubilisant pour le calcium et le magnésium, comme décrit dans le brevet   américain   n 
2.996.372, par exemple une matière contenant du sucre, no-   tamment   les mélasses résiduaires, le glucose, le fructose, le dextrose, les sirops ou analogues, avec une faible quan- tité d'un sel d'un acide   minéral   d'un métal alcalin ou 

 <Desc/Clms Page number 4> 

 alcalino-terreux tel que le chlorure de   calcium   en une   quan-   tité inférieure à environ 1%.

   On peut également ajouter une   .   faible quantité   d'un   hydroxyde ou d'un oxyde de métal alca- lin tel que l'hydroxyde de sodium, de préférence dans l'in- tervalle d'environ 0,1 à environ 1,5%. 



   Lors de la mise en oeuvre de la présente inven- tion, on obtient un produit ayant une haute résistance après avoir été soumis à des températures élevées, par exemple 
1700-1900 F   (927   à   10J8 C),   ce produit présentant également un pourcentage élevé de fer réduit après ce chauffage, ce qui indique que le produit est auto-réducteur. Ces deux propriétés sont vivement recherchées et difficiles à obtenir, 
La mise en oeuvre de la présente invention pourra être mieux comprise en se référant aux exemples suivants illustrant les points importante de l'invention.       



   EXEMPLE I 
On a pratiqué une série de tests sur des pastil-      les on transformant, en boulets, de   l'hématite   spéculaire "telle qu'elle est recueillie" et rebroyée avec du charbon      à haute teneur en produits volatils et du charbon à faible teneur en produits volatils, ainsi que des mélanges des doux types de charbon avec de la chaux, 0,5% de mélasses résiduaires et 0,4% de chlorure de calcium. On a employé le charbon "tel quel" et, dans ce cas, sa dimension était de-4 mailles, puis ii a été rebroyé à 100 mailles (100   M).   



   La chaux était une poudre de chaux dolomitique   monohydratée   connue dans le commerce sous le nom de "Ohio Super spray hydrate". 



   On a effectué, de la manière suivante,   une.série   de tests afin de déterminer la résistance et les caractéris- tiques de boulets bruts, 
Test de chute: 
On laisse tomber individuellement 20 boulets 

 <Desc/Clms Page number 5> 

   #     bruts   humides soigneusement tries de   -13/J2"     +12/32"     (-10,319mm   +9,525mm) d'une hauteur de 18 pouces   (457,2   mm) sur une plaque d'acier et l'on utilise le nombre de chutes consécutives nécessaires pour provoquer la rupture, afin de déterminer une moyenne arithmétique. 



  Test de compression de boulets brutes 
On utilise un échantillon identique à celui   du'*-   crit ci-dessus, on applique une charge de compression aux boulets individuels et l'on utilise la charge requise pour provoquer la rupture, afin de déterminer lu moyenne arithmé- tique. 



   Les résultats obtenus sont repris au tableau 1. 

 <Desc/Clms Page number 6> 

 



    TABLEAU I RESISTANCES DE BOULETS BRUTS   
 EMI6.1 
 
<tb> Type <SEP> de <SEP> Charbon <SEP> Hématite <SEP> spéculaire <SEP> Hématite <SEP> spéculaire <SEP> Chaux <SEP> Test <SEP> de <SEP> chute, <SEP> Compression <SEP> jusqu'à
<tb> charbon <SEP> % <SEP> conc. <SEP> telle <SEP> quelle <SEP> conc.rebroyée <SEP> % <SEP> chutes <SEP> jusqu'à <SEP> la <SEP> rupture
<tb> % <SEP> % <SEP> la <SEP> rupture <SEP> livres <SEP> kg
<tb> 
 
 EMI6.2 
 Charbon h.mte teneur 71,00 24,oo 5,00 6' 2,2 o ,998 CI);trbort i*i h,ute teneur en produits volatils, tel est recueilli 9,48 64,10 21 ' 30 5,12 1,3 3,3 1.497 "-tOO'M Y,7j 67,60 ' 22,,54 5,12 14 3.3 1 497 " "9,1.8 64,10 21,:30 5,12 16 4,1 1,859 " " " 18,96 56,96 18,96 5,12 24 :

  ),4 1*542 " " "25,00 52,42 17,46 5, 12 40 3,2 1,'+51 Charbon à faible teneur 2D,00 52,42 17,46 5,12 4o 'li5l 
 EMI6.3 
 
<tb> en <SEP> produits <SEP> volatils,
<tb> tel <SEP> qu'il <SEP> est <SEP> recueilli <SEP> 9,48 <SEP> 64,10 <SEP> 21,30 <SEP> 5,12 <SEP> 16 <SEP> 3,1 <SEP> 1,406
<tb> 
 
 EMI6.4 
 -100 M 9,h8 64 > 10 21 ,30 ' 5, 12 18 4,1 1 ,8iÔ*t 
 EMI6.5 
 
<tb> Charbon <SEP> à <SEP> haute <SEP> teneur
<tb> 
 
 EMI6.6 
 en produits vol<1.tils, -'..*; - 100 Il,00 8 néant 5 , 1 2 13 13 ' "8,00 85,00 néant 7,00 19 3,6 1,6J2 

 <Desc/Clms Page number 7> 

 
EXEMPLE II 
On a   traité   les pastilles de l'exemple I avec de l'anhydride carbonique à la température ambiante afin de durcir et transformer la chaux en carbonate in situ.

   On a testé ces pastilles durcies de la   marlère   suivante : Test au tambour: 
On remue une charge   de 5   livres (2,268 kg) des pastilles achevées dans un tambour à coke A.S.T.M. et   l'on   enregistre, par un pourcentage   des 5   livres initiales, le résidu restant' sur un tamis de +1/4 pouce   (6,35   mm)   .après   280 révolutions, puis on note l'indice de résistance au tambour. 



  Test de compression! 
On prélève un échantillon de 20.pastilles de -13/32" +12/32" (-10,319mm +9,525mm) et l'on applique une charge de compression aux pastilles individuelles, puis on utilise la charge requise pour la fracture, afin de déter- miner la moyenne arithmétique. 



   Les résultats de ces tests sont repris au tableau 
II.      

 <Desc/Clms Page number 8> 

 
 EMI8.1 
 
<tb> 



  Charbon <SEP> Types <SEP> de <SEP> Hématite <SEP> spéculaire <SEP> Taconite <SEP> Hydrate <SEP> de <SEP> chaux <SEP> Test <SEP> de <SEP> compression <SEP> Test <SEP> au <SEP> tambour
<tb> charbons <SEP> cône., <SEP> % <SEP> 0/0+1/4"
<tb> % <SEP> charbons <SEP> telle <SEP> quelle- <SEP> rebroyée <SEP> % <SEP> livres <SEP> kg <SEP> 280 <SEP> révolutions <SEP> 
<tb> 4,74 <SEP> Haute <SEP> teneur <SEP> en <SEP> 67,60 <SEP> 22,54 <SEP> 5,12 <SEP> 320 <SEP> 145,1 <SEP> 99
<tb> produitsvolatils <SEP> - <SEP> 100 <SEP> M
<tb> 9,48 <SEP> Haute <SEP> teneur <SEP> en <SEP> 64,10 <SEP> 21,30 <SEP> 5,12 <SEP> 225 <SEP> 102,05 <SEP> 99
<tb> produitsvolatils <SEP> - <SEP> 100 <SEP> M <SEP> 
<tb> 18,96 <SEP> Haute <SEP> teneur <SEP> en <SEP> 56,92 <SEP> 18,96 <SEP> 5,12 <SEP> 105 <SEP> 47,6 <SEP> 96
<tb> produits <SEP> volatils <SEP> - <SEP> 100 <SEP> M
<tb> 25,

  00 <SEP> Haute <SEP> teneur <SEP> en <SEP> 52,42 <SEP> 17,46 <SEP> 5,12 <SEP> 50 <SEP> 22,6 <SEP> 96
<tb> produits <SEP> vola- <SEP> 22,6
<tb> tils <SEP> - <SEP> 100 <SEP> M
<tb> 9,48 <SEP> Faible <SEP> teneur <SEP> en <SEP> 64,10 <SEP> 21,30 <SEP> 5,12 <SEP> 170 <SEP> 77,1 <SEP> 99
<tb> produitsvolatils
<tb> - <SEP> 100 <SEP> M <SEP> 
<tb> 9,48 <SEP> Haute <SEP> teneur <SEP> en <SEP> 64,10 <SEP> 21,30 <SEP> 5,12 <SEP> 250 <SEP> 113,4 <SEP> 99
<tb> produits <SEP> volatils, <SEP> tel <SEP> quel
<tb> 9,48 <SEP> Faible <SEP> teneur <SEP> en <SEP> 64,10 <SEP> 21,30 <SEP> 5,12 <SEP> 225 <SEP> 102,05 <SEP> 98
<tb> produits <SEP> volatils, <SEP> tel <SEP> quel
<tb> 10,00 <SEP> Haute <SEP> teneur <SEP> en <SEP> 84,00 <SEP> 0 <SEP> 6,00 <SEP> 260 <SEP> 117,9 <SEP> 98
<tb> produits <SEP> vola- <SEP> 0,00 <SEP> 260 <SEP> 117,9 <SEP> 98
<tb> 
 
 EMI8.2 
 tils - 100 ,M ' ...a 0 tils - 100 93,

  70 6,30 3I+3 155,5 96 1 ttt 1 1 
 EMI8.3 
 
<tb> 0 <SEP> 80,90 <SEP> 9,10 <SEP> 445 <SEP> 201,8
<tb> 5 <SEP> Haute <SEP> teneur <SEP> en <SEP> 90,00 <SEP> 5,00 <SEP> 205 <SEP> 92,9
<tb> produits <SEP> vola- <SEP> 205 <SEP> 92,9
<tb> tils <SEP> - <SEP> 100 <SEP> M
<tb> 
 

 <Desc/Clms Page number 9> 

   DONNEES DE RESISTANCE A LA TEMPERATURE AMBIANTE   
 EMI9.1 
 
<tb> Charbon <SEP> Types <SEP> de <SEP> Hématite <SEP> spéculaire <SEP> Taconite <SEP> Hydrate <SEP> de <SEP> chaux <SEP> Test <SEP> de <SEP> compression <SEP> Test <SEP> au <SEP> tambour
<tb> charbons <SEP> conc., <SEP> % <SEP> % <SEP> livres <SEP> 0/0+1/4"
<tb> % <SEP> charbons <SEP> telle <SEP> quelle <SEP> - <SEP> rebroyée <SEP> 'livres <SEP> kg <SEP> 280 <SEP> révolutions <SEP> 
<tb> 5 <SEP> Haute <SEP> teneur <SEP> en <SEP> 89,00 <SEP> 6,00 <SEP> 255 <SEP> 115,

  6 <SEP> 99
<tb> produits <SEP> vola-.
<tb> tils <SEP> - <SEP> 100 <SEP> M
<tb> 5 <SEP> Haute <SEP> teneur <SEP> en <SEP> 88,00 <SEP> 7,00 <SEP> 323 <SEP> 146,5
<tb> produits <SEP> volatils <SEP> - <SEP> 100 <SEP> M
<tb> 9,48 <SEP> 50/50 <SEP> haute <SEP> 64,10 <SEP> 21,30 <SEP> 5,12 <SEP> 205 <SEP> 92,9 <SEP> 99
<tb> -100 <SEP> hauté <SEP> teneur <SEP> en <SEP> produits <SEP> volatils/
<tb> -100 <SEP> faible <SEP> teneur <SEP> en <SEP> produitsvolatils
<tb> 9,48 <SEP> 50/50 <SEP> tel <SEP> quel <SEP> 64,10 <SEP> 21,30 <SEP> 5,12 <SEP> 24o <SEP> 108,8 <SEP> 98 <SEP> des
<tb> haute <SEP> teneur <SEP> en
<tb> 'produits <SEP> volatils <SEP> et <SEP> faible <SEP> .

   <SEP> 
<tb> teneur <SEP> en <SEP> produits <SEP> volatils
<tb> 
 

 <Desc/Clms Page number 10> 

 
EXEMPLE III
On a testé les pastilles carbonatées de l'exemple II à des températures élevées et dans des atmosphères réductrices de la manière suivante, puis on les a comparées avec une pastille commerciale de taconite durcie à la chaleur. 



  Test à la flamme vive:
On a placé des échantillons choisis sur une   toile     métallique   en fils de   nichrome   située   à 10   mm au-dessus de   l@   grille d'un brûleur de Fisher et l'on a laissé les flammes formées envelopper l'échantillon pendant une période de deux heures, après quoi on a retiré les échantillons et l'on a pratiqué une observation qualitative de leur état, Test au creuset!
On   a   placé, quatre à la fois, des pastilles soigneusement triées de   -13/32"     +12/32"   (-10,319 mm   +9,.525mm)   dans un creuset rempli de charbon, puis on a recouvert ce dernier et on l'a chauffé au moyen d'un brûleur de   Fishor   pendant une période prédéterminée,

   après quoi on a retiré les pastilles et on les a laissé retomber à la température ambiante avant de les soumettre à un test de compression jusqu'à destruction. On a répété ce cycle pendant diffé- rents cycles de durée/température, indiqués pour chaque essai. 



   Test de réduction:
On place, dans un champ magnétique, les pastilles qui ont été chauffées dans le test au creuset décrit ci- dessus, puis, en guise dtobservation qualitative, on enre- gistre le degré d'attraction. 



   Les résultats sont repris au tableau III. 

 <Desc/Clms Page number 11> 

 
 EMI11.1 
 
<tb> 



  Charbon <SEP> Hématite <SEP> spéculaire <SEP> Taconite <SEP> Hydrate <SEP> de <SEP> chaux <SEP> Test <SEP> au <SEP> creuset <SEP> - <SEP> charge <SEP> jusqu'à <SEP> la
<tb> %-type <SEP> conc.,% <SEP> % <SEP> % <SEP> rupture, <SEP> livres <SEP> après <SEP> durée <SEP> en <SEP> minutes
<tb> telle <SEP> quelle <SEP> - <SEP> rebroyée <SEP> 0 <SEP> 15 <SEP> 30 <SEP> 45 <SEP> 60 <SEP> 90 <SEP> 210
<tb> Néant <SEP> 72 <SEP> 23 <SEP> 5,00 <SEP> 410 <SEP> 23 <SEP> 14 <SEP> 9 <SEP> 8 <SEP> 11 <SEP> 12
<tb> kg <SEP> 185,9 <SEP> 10,4 <SEP> 6,3 <SEP> 4 <SEP> 3,6 <SEP> 4,9 <SEP> 5,4
<tb> 4,74-haute <SEP> teneur <SEP> en <SEP> 67,6 <SEP> 22,54 <SEP> 5,12 <SEP> 320 <SEP> 30 <SEP> 30 <SEP> 29 <SEP> 29 <SEP> 29 <SEP> 27
<tb> produits <SEP> volatils <SEP> kg <SEP> 145,1 <SEP> 13,6 <SEP> 13,6 <SEP> 13,1 <SEP> 13,1 <SEP> 13,1 <SEP> 12,

  2
<tb> - <SEP> 100 <SEP> M <SEP> 500 <SEP> 23 <SEP> 15 <SEP> 16 <SEP> 19 <SEP> 12 <SEP> 18
<tb> Pastille <SEP> de <SEP> taconite <SEP> durcies <SEP> à <SEP> la <SEP> chaleur <SEP> kg <SEP> 226,8 <SEP> 10,4 <SEP> 6,8 <SEP> 7,2 <SEP> 8,6 <SEP> 5,4 <SEP> 8,1
<tb> 9,48-haute <SEP> teneur <SEP> en <SEP> 64,1 <SEP> 21,3 <SEP> 5,12 <SEP> 250 <SEP> 27 <SEP> 27 <SEP> 24 <SEP> 22 <SEP> 22 <SEP> 19
<tb> produits <SEP> volatils, <SEP> kg <SEP> 113,4 <SEP> 12,2 <SEP> 12,2 <SEP> 10,8 <SEP> 9,9 <SEP> 9,9 <SEP> 8,6
<tb> tel <SEP> quel
<tb> 9,48-haute <SEP> teneur <SEP> en <SEP> 64,1 <SEP> 21 <SEP> ,3 <SEP> 5,12 <SEP> 225 <SEP> 30 <SEP> 30 <SEP> 30 <SEP> 30 <SEP> 29 <SEP> 21
<tb> produits <SEP> volatils <SEP> kg <SEP> 102.- <SEP> 13,6 <SEP> 13,6 <SEP> 13,6 <SEP> 13,6 <SEP> 13,1 <SEP> 9,5
<tb> - <SEP> 100 <SEP> M
<tb> 9,48-haute <SEP> teneur <SEP> en <SEP> 34,2 <SEP> 51,20 <SEP> 5,

  12 <SEP> 180 <SEP> 30 <SEP> 30 <SEP> 30 <SEP> 30 <SEP> 30 <SEP> 27
<tb> produits <SEP> volatils <SEP> kg <SEP> 81,6 <SEP> 13,6 <SEP> 13,6 <SEP> 13,6 <SEP> 13,6 <SEP> 13,6 <SEP> 12,2
<tb> - <SEP> 100 <SEP> M
<tb> 9,,48-faible <SEP> teneur <SEP> en <SEP> 64,1 <SEP> 21,3 <SEP> 5,12 <SEP> 30 <SEP> 25 <SEP> 21 <SEP> 20 <SEP> 20 <SEP> ...17:

  
<tb> 'produits <SEP> volatils, <SEP> kg <SEP> 13,6 <SEP> 11,3 <SEP> 9,5 <SEP> 9.- <SEP> 9.- <SEP> 7,7
<tb> tel <SEP> quel
<tb> 18,96-haute <SEP> teneur <SEP> en <SEP> 56,96 <SEP> 18,96 <SEP> 5,12 <SEP> 105 <SEP> 30 <SEP> 23 <SEP> 23 <SEP> 17 <SEP> 15 <SEP> 10
<tb> produits <SEP> volatils <SEP> kg <SEP> 47,6 <SEP> 13,6 <SEP> 10,4 <SEP> 10,4 <SEP> 7,7 <SEP> 6,8 <SEP> 4,5
<tb> - <SEP> 100 <SEP> M
<tb> 11,00-haute <SEP> teneur <SEP> en <SEP> 83,88 <SEP> 5,12 <SEP> 160 <SEP> 30 <SEP> 28 <SEP> 23 <SEP> 20 <SEP> 19 <SEP> 12
<tb> produits <SEP> volatils <SEP> kg <SEP> 72,5 <SEP> 13,6 <SEP> 12,7 <SEP> 10,4 <SEP> 9.- <SEP> 8,6 <SEP> 5
<tb> - <SEP> 100 <SEP> M
<tb> 1300-haute <SEP> teneur <SEP> 1,88,12 <SEP> 135 <SEP> ...
<tb> t3,00-haute <SEP> teneur <SEP> en <SEP> 81,88 <SEP> 5,12 <SEP> 135 <SEP> 30 <SEP> 30 <SEP> 29 <SEP> 25 <SEP> 22
<tb> produits <SEP> volatils <SEP> kg <SEP> 61,

  2 <SEP> 13,6 <SEP> 13,6 <SEP> 13,1 <SEP> 11,3 <SEP> 9,9 <SEP> 7,2
<tb> - <SEP> 100 <SEP> M
<tb> Néant <SEP> 70,0 <SEP> 23,5 <SEP> 6,50 <SEP> 500 <SEP> 30 <SEP> 26 <SEP> 23 <SEP> 16 <SEP> 19 <SEP> 17
<tb> kg <SEP> 226,8 <SEP> 13,6 <SEP> 11,7 <SEP> 10,4 <SEP> 7,2 <SEP> 8,6 <SEP> 7,7
<tb> 
 

 <Desc/Clms Page number 12> 

 
 EMI12.1 
 DU'\r;5 DU TEST .kC' .C#C6ET 
 EMI12.2 
 Charbon Fiêmatite spéculaire Taconite Hydrate de chaux Test'u creuset - Ch1rge jusqu'à la %-type conc.,% , ;o rupture, livres 'près durée en mÍt1utes telle quelle- rebroyée 0 t 30 :'5 60 <JO 2 f U 10,OO-h;1ute teneur en 84,0 6,oo 170 ,30 , 30 30 30 26. 18 produits volatils kg 77, 13,6 13,6 iJ,6 JJ,Ó Il,7 8,1 - 1 GO M t0 .

   UU-haute teneur en $ 3. 0 7,00 178 30 .30 30 30 2h 22 produits volatils kg 80,7 13,6 13,6 1.3,6 IJ,6 12,7 9,9 - 100 101 80,7 t3,G y,c t3,6 t3,6 l,i Néant 57oO J8,0 5,00 11 5 ,S 8 8' 9 9 (non carboné) kg 4,9 2,2 3,6 3,6 3,6 t.- t.-. 



  9,ll8 51,2 34,z 5, 12 5 5 3 2 2 3 3 (non carboné) kg 2,2 2,2 1#3 0,9 0,9 1,3 1,3 Néant 60 .0 Néant 10 ' z 2 2 2 2 . 



  (non carboné) kg 4,5 0,9 0,'9 0,9 . 0,9 U,9 0:9 (0,75 de bentonite) 1...1. 



  1 ù 

 <Desc/Clms Page number 13> 

 EXEMPLE IV 
On a   forme   des pastilles comme décrit à l'exemple II par carbonatation en remplaçant   l'hématite   spéculaire par des concentrais de taconite. On a soumis ces pastilles aux mêmes tests que ceux de l'exemple III. Les données sont reprises au tableau IV. 

 <Desc/Clms Page number 14> 

 



    TABLEAU IV   
 EMI14.1 
 
<tb> Charbon <SEP> Hématite <SEP> spéculaire <SEP> Taconite <SEP> Hydrate <SEP> de <SEP> chaux <SEP> Test <SEP> au <SEP> creuset <SEP> - <SEP> charge <SEP> Jusqu'à <SEP> la
<tb> 56-type <SEP> conc.,% <SEP> % <SEP> % <SEP> rupture, <SEP> livres <SEP> après <SEP> durée <SEP> en <SEP> minutes
<tb> ¯¯¯¯¯¯¯¯¯¯¯¯¯¯¯¯ <SEP> telle <SEP> quelle- <SEP> rebroyée <SEP> 0 <SEP> 15 <SEP> 30 <SEP> 45 <SEP> 60 <SEP> 90 <SEP> 210
<tb> Néant <SEP> 93,7 <SEP> 6,3 <SEP> 343 <SEP> 30 <SEP> 30 <SEP> 30 <SEP> 30 <SEP> 30 <SEP> 30
<tb> kg <SEP> 155,5 <SEP> 13,6 <SEP> 13,6 <SEP> 13,6 <SEP> 13,6 <SEP> 13,6 <SEP> 13,6
<tb> 5,00-haute <SEP> teneur <SEP> en <SEP> 88,0 <SEP> 7,0 <SEP> 323 <SEP> 50 <SEP> 40 <SEP> 30 <SEP> 30 <SEP> 30 <SEP> 30
<tb> produits <SEP> volatils <SEP> kg <SEP> 146,4 <SEP> 22,6 <SEP> 18,1 <SEP> 13,6 <SEP> 13,6 <SEP> 13,6 <SEP> 13,

  6
<tb> - <SEP> 100 <SEP> M
<tb> Néant <SEP> 93,28 <SEP> 6,72 <SEP> 10 <SEP> 16 <SEP> 25 <SEP> 28 <SEP> 20 <SEP> 13 <SEP> 19
<tb> (non <SEP> carboné) <SEP> kg <SEP> 4,5 <SEP> 7,2 <SEP> 11,3 <SEP> 12,7 <SEP> 9,0 <SEP> 5,8 <SEP> 8,6
<tb> 9,48-haute <SEP> teneur <SEP> en <SEP> 83,80 <SEP> 6,72 <SEP> 7 <SEP> 8 <SEP> 7 <SEP> 9 <SEP> 7 <SEP> 6 <SEP> 8
<tb> produits <SEP> volatils <SEP> (non <SEP> carboné) <SEP> kg <SEP> 3,1 <SEP> 3,6 <SEP> 3,1 <SEP> 4,0 <SEP> 3,1 <SEP> 2,7 <SEP> 3,6
<tb> - <SEP> 100 <SEP> M
<tb> 
 

 <Desc/Clms Page number 15> 

 
EXEMPLE V 
On a formé des pastilles en mélangeant de l'hy- drate de chaux, du charbon et un minerai comme décrit à l'exemple I.

   On a soumis les pastilles   forthées   à une   atinos-          phère   d'anhydride carbonique suffisante pour former de la pierre à chaux recristallisée in situ. On a ensuite divisé les pastilles carbonatées en deux parties, une partie étant chauffée à   1600 F     (871 C)   et l'autre, à 1700 F (927 C) dans une atmosphère contenant de l'oxyde de carbone analogue à celle que l'on rencontrerait dans un haut fourneau ou un four analogue de traitement du fer. On a retiré les pastil- les et on les a analysées pour déterminer la teneur en fer réduit. Les résultais sont repris au tableau V. 

 <Desc/Clms Page number 16> 

 



    TABLEAU V PASTILLES LIEES AU CARBONATE   
 EMI16.1 
 
<tb> Réduction, <SEP> %
<tb> 1600 F <SEP> 1700 F
<tb> Concentra <SEP> de <SEP> taconite <SEP> (871 C) <SEP> (927 C)
<tb> 6% <SEP> d'hydrate <SEP> de <SEP> chaux <SEP> 38,7 <SEP> 44,8
<tb> 9% <SEP> d'hydrate <SEP> de <SEP> chaux <SEP> -
<tb> 12% <SEP> d'hydrate <SEP> de <SEP> chaux
<tb> 6% <SEP> d'hydrate <SEP> de <SEP> chaux <SEP> + <SEP> 5% <SEP> de <SEP> charbon <SEP> 49,1 <SEP> 81,5
<tb> à <SEP> haute <SEP> teneur <SEP> en <SEP> produits <SEP> volatils <SEP> (-100 <SEP> M) <SEP> - <SEP> -' <SEP> 
<tb> 9% <SEP> d'hydrate <SEP> de <SEP> chaux <SEP> + <SEP> 8% <SEP> de <SEP> charbon <SEP> à <SEP> haute <SEP> teneur <SEP> en <SEP> produits
<tb> volatils <SEP> + <SEP> 2% <SEP> de <SEP> charbon <SEP> à <SEP> faible <SEP> teneur <SEP> en <SEP> produits <SEP> volatils <SEP> (-8 <SEP> M)

   <SEP> - <SEP> Concentrat <SEP> d'hématite <SEP> spéculaire
<tb> 23,5% <SEP> d'hématite <SEP> spéculaire <SEP> rebroyée <SEP> (-325 <SEP> M) <SEP> 39,3 <SEP> 45,6
<tb> + <SEP> 5% <SEP> d'hydrate <SEP> de <SEP> chaux
<tb> 23% <SEP> d'hématite <SEP> spéculaire <SEP> rebroyée <SEP> (-325 <SEP> M) <SEP> + <SEP> 55% <SEP> d'hydrate <SEP> 50,6 <SEP> 74,1
<tb> de <SEP> chaux <SEP> + <SEP> 5% <SEP> de <SEP> charbon <SEP> à <SEP> haute <SEP> teneur <SEP> en <SEP> produits <SEP> volatils <SEP> 39,8 <SEP> Hématite <SEP> spéculaire <SEP> telle <SEP> quelle <SEP> + <SEP> 5% <SEP> d'hydrate <SEP> de <SEP> ch<xux <SEP> 49,1 <SEP> 87,1
<tb> + <SEP> 10% <SEP> de <SEP> charbon <SEP> à <SEP> haute <SEP> teneur <SEP> en <SEP> produits <SEP> volatils
<tb> Minerai <SEP> du <SEP> Vénézuela
<tb> Minerai <SEP> du <SEP> Vénézuela <SEP> -3/8 <SEP> pouce <SEP> (-9,525mm)

   <SEP> + <SEP> 15% <SEP> de <SEP> charbon <SEP> à <SEP> hauteteneur <SEP> en <SEP> produits <SEP> volatils <SEP> (-100 <SEP> M) <SEP> + <SEP> 6% <SEP> d'hydrate <SEP> de <SEP> chaux
<tb> 
 

 <Desc/Clms Page number 17> 

 . EXEMPLE VI
On a formé une autre série de pastilles comme décrit   à   l'exemple V et, après les avoir retirées du four de chauffage à 1600 F   (871 C)   et 1700 F   (927 C)   respectivement, on les a   taniisées   pour déterminer la quantité de plus de 4 mailles et   la   quantité de moins de 20 mailles. On les a ensuite fait vibror pendant 15 minutes dans un récipient et on les a à nouveau tamisées. Los résultats du test sont repris au tableau VI. 

 <Desc/Clms Page number 18> 

 



    TABLEAU VI   
 EMI18.1 
 
<tb> Test <SEP> de <SEP> tamisage <SEP> après <SEP> Test <SEP> de <SEP> tamisage <SEP> après
<tb> traitement <SEP> au <SEP> four <SEP> vibration
<tb> 
 
 EMI18.2 
 16000P(8710c) 1700oF{97 C) i6oooF{S710C) 1700or'{927 C) +4M -20M +4  -20M +4b1 -20M +4M -20M 
 EMI18.3 
 
<tb> Taconite
<tb> 6% <SEP> d'hydrate <SEP> de <SEP> chaux <SEP> 96,7 <SEP> 1,67 <SEP> 96,9 <SEP> 1,48 <SEP> - <SEP> - <SEP> 43,7 <SEP> 51,8
<tb> 
 
 EMI18.4 
 9 d'hydrate de chaux 9919 0,1 99,87 0113 77,82 21,96 78,28 21,62 12% d'hydrate de chaux 99,6 013 99,5 0,2 8319 1519 82,8 16,8 g, â d'hydrate de chaux + 10;

  o de charbon à haute 99,2 O,J8 97,6 0,13 80,64 17,JO 80,09 15,0 
 EMI18.5 
 
<tb> teneur <SEP> en <SEP> produits <SEP> volatils <SEP> (-8 <SEP> M)
<tb> 9% <SEP> d'hydrate <SEP> de <SEP> chaux <SEP> + <SEP> 8% <SEP> de <SEP> charbon <SEP> à <SEP> haute <SEP> 98,62 <SEP> 0,61 <SEP> 99,47 <SEP> 0,23 <SEP> 81,00 <SEP> 16,98 <SEP> 84,17 <SEP> 14,24
<tb> teneur <SEP> en <SEP> produits <SEP> volatils(-8 <SEP> M) <SEP> et <SEP> 2% <SEP> de <SEP> charbon
<tb> à <SEP> faible <SEP> teneur <SEP> en <SEP> produits <SEP> volatils <SEP> (-8 <SEP> M) <SEP> bzz
<tb> 
 
 EMI18.6 
 9% d'hydrate de chuux + 8fi de charbon à haute 96,69 0,56 98,57 , 81,77 14,23 78o,77 ?,37 
 EMI18.7 
 
<tb> teneur <SEP> en <SEP> produits <SEP> volatils <SEP> (-8 <SEP> + <SEP> 150 <SEP> M)

   <SEP> et <SEP> 2% <SEP> de
<tb> charbon <SEP> à <SEP> faible <SEP> teneur <SEP> en <SEP> produits <SEP> volatils
<tb> (-8 <SEP> + <SEP> 150 <SEP> M)
<tb> 
 
 EMI18.8 
 iI<Ùni tite spécuiaire H<nuKitite spéctilaire 25% d'hématite spéculaire rebroyée (-325 kl) + ,5,6 99,60 0135 96,80 z,54 76,77 20,17 57,12 :)6, I;i 
 EMI18.9 
 
<tb> d'hydrate <SEP> de <SEP> chaux <SEP> + <SEP> 15% <SEP> de <SEP> charbon <SEP> à <SEP> haute
<tb> teneur <SEP> en <SEP> produits <SEP> volatils <SEP> (-100 <SEP> M)
<tb> 
 
 EMI18.10 
 Hincrai du Vénezuela l  1 ,',Iineraî Véne>zuela 97,59 0,8'7 6o,4 ¯3 :)2,4 1 + 4,76 d'hydrate de chaux 97,59 0,87 - - 60,4J J2,41 ù . 1 6;b d'hydrate de chaux + 15, de charbon à haute 98,0 1,0 95,4 2,0 85'70 11,79 8,75 .

   Zi$2 
 EMI18.11 
 
<tb> teneur <SEP> en <SEP> produits <SEP> volatils <SEP> (-100 <SEP> M)
<tb> 
 

 <Desc/Clms Page number 19> 

 
D'après les tableaux et les exemples ci-dessus, il est évident   que,.par   la mise en oeuvre de   la   présente invention, on peut obtenir une pastille de haute résistance pouvant avoir un haut niveau   d'auto-réduction.   



   Bien que l'on ait décrit certaines formes de réalisation et certains produits préférés suivant l'invention, il est entendu que l'invention peut être mise en oeuvre      d'une autre manière dans le cadre des revendications   ci-   après. 



   REVENDICATIONS 
 EMI19.1 
 A.....,".¯aoa.,.m,..... 



   1.Procédé de fabrication d'un minorai agglomère à haute résistance et auto-réducteur à partir de matières finement divisées contenant du fer, caractérisé en ce qu'il comprend les étapes consistant à mélanger la matière finement divisée contenant du minorai métallique avec au moins un élément du groupe comprenant les oxydes et les hydroxy-   des   des métaux   alcalino-terreux,   ainsi qu'avec une matière   ca.rbonée   choisie parmi le groupe comprenant le charbon, le coke, le graphite, le menu coke et le charbon de bois, transformer le mélange en agglomérés   et.faire   réagir les agglomérés avec de l'anhydride carbonique en présence d'humidité, pour former des carbonates   alcalino-terreux   in situ dans les agglomérés.

Claims (1)

  1. 2. Procédé suivant la revendication 1, caracté- risé en ce que la matière carbonée est du charbon ayant une finesse de 4 mailles et moins.
    3. Procédé suivant la revendication 1, caracté- risé en ce qu'on ajoute jusqu'à environ 2% en poids d'un agent solubilisant pour les métaux alcaline-terreux, calcu- lés sur le mélange total.
    4. Procédé suivant la revendication 1, caracté- <Desc/Clms Page number 20> risé en ce qu'on ajoute un sel d'un acide minéral choisi parmi le groupe comprenant les métaux alcalins et alcalino- terreux en une quantité allant jusqu'à environ 1%, calculé sur le poids du mélange.
    5. Procédé de fabrication d'un minerai aggloméré à haute résistance et auto-réducteur à partir de matières finement divisées contenant un métal, caractérisa en ce qu'il comprend les étapes qui consistent à mélanger la.
    méfiera finement divisée contenant un métal avec au moins un des éléments du groupe comprenant les oxydes et les hy- droxydes des totaux alcalino-terreux, ainsi qu'avec une matière carbonée choisie parmi le groupe comprenant le char- bon, le coke, le graphite, le menu coke et le charbon de bois, y ajouter jusqu'à environ 2% d'un agent solubilisant pour le magnésium et le calcium jusqu'à environ 1% d'un sel d'un acide minéral d'un membre choisi parmi le groupe compre- nant les métaux alcalins et les métaux alcalino-terreux,
    ainsi qu'environ 0,1 à environ 1,5% d'un membre choisi parmi le groupe comprenant les oxydes et les hydroxyde.,3 de métaux ! alcalins, transformer le mélange en agglomérés et :raire les agglomérés avec de l'anhydride carbonique en présence d'humidité, pour former des carbonates alcalino- terreux in situ dans les agglomères.
    6. Procède suivant la revendication 5, caracté- risé en ce que la teneur en humidité du mélange est infé- rieure à environ 10% en poids, calculés sur le mélange total.
    7. Procédé de fabrication de minerais agglomérés à haute résistance et auto-réducteurs à partir de matières finement divisées contenant du fer, caractérisé en ce qu'il comprend les étapes qui consistent à mélanger la matière finement divisée contenant du fer avec environ 5 à 20% d'au nioins un membre choisi parmi le groupe comprenant les <Desc/Clms Page number 21> .. EMI21.1 oxydes et les hydroxydes des ar!t"mv ;!fc.:ïi,rac-.taxroux t't uvée environ 1 à 35% drurtt" ni,<t,1">r<. t': tlUatln <;1>nisii; 1.I,'l'Hll le groupe comprenant le cls;,rtaa,r,, le coke, ii:
    ,I,!l11 Qokc, tf graphite et le churtjon do bols, tl'aus!'or'l!ler 1t rattl.cn,;E3 art ul.oriacrés ot faire r.);I{;ir Jcs ,.[';{r 1 Om':!";S .,V.)C do 1 t.m!ly.dride carbonique en prusonco d'humiditt'' pou' {'oJ'I1tn' dus. carbonates alcaxlino..torrfaux ln situ d.!rlrs liai; =xggl<>ntt";<tsg 8. Proc4<Iô suivant la r<a,<oiidic<.it,1r-n 7 c r.:ct,(riso on co qu'on incorpore, HU 1t161."II'Ot JUSqU';'1 env1rolt ;7.';' d'un éJ.lent solubilisunb pour Le calcium ei: iu lad{:!1,S::;l\1rn.
    9. Procédé do fabrication d'un ijilttpr -4i de t'or lf;fFJomvr â hüutc résistance 4uiEi;>iit: 1;= i'à,,ondic;it-J.uii 7 , caractérise en co que la /IIHtiiJre c;!rbonta est; le charbon.
    10. Procodu de fabrication d'un minerai de fer aggloméré à haute résistance suivant 1.;i revendication 7, caractérisa en co que le mÓllIIGo eontiont jusqu'à environ 10,c'o' d'humidité.
BE712285D 1968-03-15 1968-03-15 BE712285A (fr)