CH160761A - Process for the production of pellets. - Google Patents

Process for the production of pellets.

Info

Publication number
CH160761A
CH160761A CH160761DA CH160761A CH 160761 A CH160761 A CH 160761A CH 160761D A CH160761D A CH 160761DA CH 160761 A CH160761 A CH 160761A
Authority
CH
Switzerland
Prior art keywords
parts
condensation
filler
pressed
formaldehyde
Prior art date
Application number
Other languages
German (de)
Inventor
Gesellschaft Fuer Chemis Basel
Original Assignee
Chem Ind Basel
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Chem Ind Basel filed Critical Chem Ind Basel
Publication of CH160761A publication Critical patent/CH160761A/en

Description

  

      Verfahren    zur Herstellung von     Presslfngen.            DieVerfahren    der Patente Nr. 125729 und       7-16i009,    sowie der Zusatzpatente Nr.     141223,          142936    und 14d22(1 beschreiben die Herstel  lung von     Kondensationsprodukten    aus aroma  tischen Aminen und Aldehyden. die sich mit  oder ohne Zusatz von Füllstoffen.     Härtungs-          mitteln,    Farbstoffen,     Weichmachungsmitteln          usw.    unter Hitze und Druck verformen  lasen.  



       Füllstoffhaltige    Formstücke     sind        iunso     wertvoller, je homogener die     Mischung    des       Bindernittel:s    mit dem Füllstoff durchgeführt  wird. So sind die gemäss Patent Nr. 1,42936       rbzrch    Ausfällen des Kondensationsproduktes  in und auf dem Füllmittel erhaltenen     Press-          mischungen    homogener als die durch blosses  Zusammenmahlen der Komponenten erhal  tenen Produkte.  



       Nach    Patent Nr. 142936 fällt das Kon  densationsprodukt in voluminöser Form aus.  Dadurch entsteht die Gefahr     einer    gewissen       Entmischun-    bei der nachfolgenden Troek-    nun- und Zerkleinerung des     füllstoffhaltigen     Kondensationsproduktes.  



  Es wurde nun ein Weg gefunden, um  die     Kondensationsprodukte-in-viel-zlichterer     Form auf den Füllstoffen niederzuschlagen.  



  Es ist bekannt, die Kondensation von  primären aromatischen     Aminen    mit Form  aldehyd in Gegenwart von Säuren so zu lei  ten,     daB    feste Gallerten entstehen, die ohne  Formänderung ausgewaschen und von Elek  trolyten befreit werden können und dann  bonnartige Produkte bilden. Es ist auch be  kannt, solchen Lösungen vor dem Erstarren  Füllstoffe beizumischen, wobei durch Erstar  ren der Masse gefüllte Formkörper entstehen       (vergl.    Patent Nr.     123,515    und Nr.     154831).     



  Wird aber das mit einer     gelatinierfähigen     Kondensationslösung getränkte Füllmaterial  während des     Gelatinierens    oder jedenfalls vor  vollständiger Erhärtung der Gallerte gerührt  oder geknetet, so erhält man eine bröckelige  Masse, die aus     kleinen        Gallertbrocken        be-          steht,-welche    die Teilchen des Füllmaterials      fest umschliessen und beim Behandeln mit       säureeliminierenden        Mitteln    nicht zerfallen;  sondern in dichter     horniger    Form     untrennbar     mit den Füllern verbunden bleiben.  



  Die kleinen -     Gallertteilchen    lassen sich  naturgemäss viel rascher auswaschen als grö  ssere Formstücke; durch Mahlen und     Ver-          pressen    der gewaschenen und getrockneten  Mischung erhält man     Presslinge    von beson  ders guter     Homogenität.     



  Besonders augenfällig ist der     Unterschied     gegenüber dem Verfahren gemäss Patent       Nr.142936,    wenn spezifisch schwere, nicht  saugfähige Füllmaterialien,     wie    Glimmer,  Schiefermehl und dergleichen, verwendet  werden. Die Gallerte vermag auch solche       Füllmittel    so zu umschliessen, dass auch beim       Zerkleinern    des Reaktionsproduktes     eine          Entmischung    nicht     eintritt    und beim Pressen  homogene     Presskörper    erhalten werden.  



  Der Zusatz der Füllstoffe kann in einer  beliebigen Phase der     Kondensation    erfolgen,  das heisst man     kann    dieselben     entweder    den  Komponenten oder der Mischung ,derselben       bezw.    der Kondensationslösung in jedem be  liebigen Stadium-vor der     Gelbildung    zufügen.  Man kann auch den Formaldehyd in bekann  ter Weise in mehreren     Stufen    zugeben.  



  Das Verfahren     wird    .durch folgende Bei  spiele     erläutert,    wobei die angegebenen Teile  Gewichtsteile sind.  



  <I>Beispiel 1:</I>  <B>130,</B> Teile     Anilinchlorhydrat    (1 Hol)  werden in 200 Teilen Wasser gelöst und       unter    Rühren mit 98 Teilen 40 %     igem    Form  aldehyd (1,2     Mol)    und     unmittelbar    darauf  mit 100 Teilen Holzmehl innig vermischt.  Durch     Aussenkühlung    wird die Temperatur  des Kondensationsgemisches unter 50   C ge  halten, und durch stetes Rühren wird die  sich     nun    bildende rote Gallerte in zerkleiner  ten Zustand gebracht.  



  Diese fein     zerkleinerte,    mit Holzmehl  gefüllte Gallerte wird nun- mit<B>400</B> Teilen       1-5%iger    Natronlauge behandelt, wobei die  Farbe von rot nach gelb umschlägt. Schliess  lich     wird    mit viel Wasser     elektrolytfrei    ge-    waschen und bei<B>70'</B> im Vakuum getrocknet.

    Das auf diese Weise     erhaltene,    hellgelbe       Presspulver    lässt sich bei 155   zu     Presslingen     von ausserordentlicher Homogenität     ver-          pressen.      <I>Beispiel 2:</I>  Zu 130 Teilen     Anilinchlorhydrat    (1     Mol),     die in 200 Teilen Wasser gelöst werden, gibt.

    man 160 Teile aufgeschlagene Zellulose  (Kraftstoff), die noch etwa<B>70%</B> Wasser  enthält und verrührt das Gemisch mit 82  Teilen 40%igem Formaldehyd (1     Mol).     Durch Kühlen wird die Temperatur unter  <B>30</B>   gehalten, und nun werden weitere  33 Teile 40%iger Formaldehyd (0,4     Mol)     zugegeben, durch stetes gutes Rühren die zur  Gallerte erstarrende Masse fein zerkleinert  und nach Beispiel 1 neutralisiert, aus  gewaschen und getrocknet. Es wird auf diese  Weise ein gelbes     Presspulver    erhalten, das,  bei<B>160'</B>     verpresst,    einen sehr homogenen       PreBling    von ausgezeichneten mechanischen  Eigenschaften darstellt.

      <I>Beispiel 3:</I>  93 Teile Anilin (1     Mol)    werden mit<B>100</B>  Teilen     86%iger    Ameisensäure und unter  gutem Rühren und Kühlen mit 82 Teilen  40%igem Formaldehyd (1     Mol)    versetzt.  Unter sehr starker Erwärmung färbt sich  das Kondensationsgemisch tiefrot. Nachdem  durch Aussenkühlung die Temperatur auf  30   gesunken ist, werden nun weitere 33  Teile 40%iger Formaldehyd (0,4     Mol)    und  zugleich     unter    sehr gutem Rühren<B>100</B> Teile  Holzmehl zugegeben. Nach wenigen Minu  ten stellt das Kondensationsprodukt eine  fein zerteilte homogene Gallerte dar. Diese  wird nach Beispiel 1 weiter zu einem hell  gelben     Presspulver    aufgearbeitet.

   Die daraus  hergestellten     Presslinge    sind sehr homogen  und haben sehr gute mechanische und elek  trische Eigenschaften.         Beispiel   <I>4:</I>  In 200 Teilen Wasser werden 130 Teile       Anilinchlorhydra.t    (1 Hol) und 100 Teile      feines     Glimmerpulver    eingetragen. Unter  gutem Rühren werden 115 Teile 40%iger       Formaldehyd        (1.,.1        NIo1)    zugegeben. Unter  starker Erwärmung bildet sich eine orange  rote Gallerte, die durch kräftiges Kneten  fein zerkleinert wird. Durch Aussenkühlung  wird die Temperatur des Kondensations  gemisches unter<B>50'</B> gehalten. Die Auf  arbeitung erfolgt auch hier nach Beispiel 1.

    Das so hergestellte     Presspulver    liefert beim       Verpressen    bei<B>160'</B> sehr homogene     Press-          linge.    Diese zeichnen sich besonders durch  ihre guten     dielektrischen    Eigenschaften aus.



      Process for the production of pressed lengths. The processes of patents no. 125729 and 7-16i009, as well as additional patents no. 141223, 142936 and 14d22 (1 describe the production of condensation products from aromatic amines and aldehydes, which are with or without the addition of fillers, hardeners, dyes Deform plasticizers, etc. under heat and pressure.



       Filler-containing moldings are more valuable, the more homogeneously the mixture of the binder: s is carried out with the filler. The press mixtures obtained according to patent no. 1,42936 rbzrch precipitations of the condensation product in and on the filler are more homogeneous than the products obtained by simply grinding the components together.



       According to patent no. 142936, the condensation product precipitates in a voluminous form. This creates the risk of a certain separation in the subsequent drying and comminution of the filler-containing condensation product.



  A way has now been found to deposit the condensation products-in-much-more-light form on the fillers.



  It is known to conduct the condensation of primary aromatic amines with formaldehyde in the presence of acids in such a way that solid jellies are formed which can be washed out and freed from electrolytes without changing their shape and then form Bonny-like products. It is also known to add fillers to such solutions before they solidify, resulting in filled moldings as a result of solidification of the mass (cf. Patent No. 123,515 and No. 154831).



  If, however, the filling material soaked with a gelatinizable condensation solution is stirred or kneaded during gelatinization or at least before the jelly has completely hardened, a crumbly mass is obtained, which consists of small chunks of jelly, which tightly surround the particles of the filler material and with the treatment acid eliminators do not disintegrate; but remain inextricably linked to the fillers in a dense, horny shape.



  The small gelatinous particles can naturally be washed out much more quickly than larger shaped pieces; by grinding and pressing the washed and dried mixture, compacts of particularly good homogeneity are obtained.



  The difference compared to the method according to Patent No. 142936 is particularly striking when specifically heavy, non-absorbent filling materials such as mica, slate flour and the like are used. The jelly can also enclose such fillers in such a way that even when the reaction product is comminuted, segregation does not occur and homogeneous pressed bodies are obtained when pressed.



  The addition of the fillers can take place in any phase of the condensation, that is, the same can either be the components or the mixture, the same respectively. add to the condensation solution at any stage before gel formation. You can also add the formaldehyde in a known manner in several stages.



  The process is illustrated by the following examples, the parts given being parts by weight.



  Example 1: 130 parts of aniline chlorohydrate (1 hol) are dissolved in 200 parts of water and, with stirring, 98 parts of 40% formaldehyde (1.2 mol) and immediately then intimately mixed with 100 parts of wood flour. The temperature of the condensation mixture is kept below 50 C by external cooling, and the red jelly that is now forming is brought into a crushed state by constant stirring.



  This finely chopped jelly filled with wood flour is then treated with <B> 400 </B> parts of 1-5% sodium hydroxide solution, the color changing from red to yellow. Finally, it is washed free of electrolytes with plenty of water and dried at <B> 70 '</B> in a vacuum.

    The light yellow press powder obtained in this way can be pressed at 155 to form tablets of exceptional homogeneity. <I> Example 2 </I> is added to 130 parts of aniline chlorohydrate (1 mol), which are dissolved in 200 parts of water.

    160 parts of whipped cellulose (fuel) which still contains about 70% water and the mixture is stirred with 82 parts of 40% formaldehyde (1 mol). The temperature is kept below <B> 30 </B> by cooling, and a further 33 parts of 40% formaldehyde (0.4 mol) are now added, the mass, which has solidified to form a gel, is finely comminuted by constant good stirring and neutralized according to Example 1 , washed off and dried. In this way, a yellow press powder is obtained which, when pressed at <B> 160 '</B>, represents a very homogeneous preBling with excellent mechanical properties.

      Example 3: 93 parts of aniline (1 mol) are mixed with 100 parts of 86% formic acid and, with thorough stirring and cooling, with 82 parts of 40% formaldehyde (1 mol) . The condensation mixture turns deep red when heated very strongly. After the temperature has fallen to 30 as a result of external cooling, a further 33 parts of 40% formaldehyde (0.4 mol) and at the same time 100 parts of wood flour are added with very good stirring. After a few minutes, the condensation product is a finely divided, homogeneous jelly. This is further worked up according to Example 1 to give a light yellow press powder.

   The pellets made from it are very homogeneous and have very good mechanical and electrical properties. Example <I> 4: </I> 130 parts of aniline chlorohydrate (1 hol) and 100 parts of fine mica powder are introduced into 200 parts of water. 115 parts of 40% strength formaldehyde (1, 1 NIo1) are added with thorough stirring. When heated strongly, an orange-red jelly forms, which is finely crushed by vigorous kneading. The temperature of the condensation mixture is kept below <B> 50 '</B> by external cooling. The work-up also takes place here according to Example 1.

    The pressed powder produced in this way delivers very homogeneous pressed parts at <B> 160 '</B>. These are particularly characterized by their good dielectric properties.

 

Claims (1)

PATENTANSPRUCH: Verfahren zur Herstellung füllstoffhal- tiger Presslinge aus füllstoffhaltigen gela- tinierfähigen sauren Lösungen von Konden sationsprodukten aus aromatischen Aminen und Aldehyden, dadurch gekennzeichnet, dass das entstehende Gel während seiner Bil dung zerkleinert, von der Säure befreit und hierauf verpresst wird. PATENT CLAIM: Process for the production of filler-containing pellets from filler-containing, gelatinizable acidic solutions of condensation products from aromatic amines and aldehydes, characterized in that the resulting gel is comminuted during its formation, freed from the acid and then pressed.
CH160761D 1932-05-04 1932-05-04 Process for the production of pellets. CH160761A (en)