CN101007732A - Natural travertine-imitated ceramic brick and making method - Google Patents

Natural travertine-imitated ceramic brick and making method Download PDF

Info

Publication number
CN101007732A
CN101007732A CN 200710026323 CN200710026323A CN101007732A CN 101007732 A CN101007732 A CN 101007732A CN 200710026323 CN200710026323 CN 200710026323 CN 200710026323 A CN200710026323 A CN 200710026323A CN 101007732 A CN101007732 A CN 101007732A
Authority
CN
China
Prior art keywords
porcelain brick
natural cavity
slurry
powder
cavity stone
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN 200710026323
Other languages
Chinese (zh)
Other versions
CN100439280C (en
Inventor
李深增
林斌
祝万里
Original Assignee
霍镰泉
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 霍镰泉 filed Critical 霍镰泉
Priority to CNB2007100263238A priority Critical patent/CN100439280C/en
Publication of CN101007732A publication Critical patent/CN101007732A/en
Application granted granted Critical
Publication of CN100439280C publication Critical patent/CN100439280C/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a ceramic brick to imitate natural cavity stone, which comprises the following parts: 8-15% ball earth, 18-30% sodium feldspar, 30-45% lithium feldspar, 12-20% limestone, 0.5-3% rubber brick material and 0-1% sintered talcum.

Description

Porcelain brick of a kind of natural cavity stone imitation and preparation method thereof
Technical field
The present invention relates to the porcelain brick production technical field; More particularly relate to have the porcelain brick and the preparation method of natural cavity stone style.
Background technology
Polished tile is a profuse architectural pottery product category, and every polishing manufacturing procedure of passing through again behind sintering makes its surface acquisition glossy product all can be polished tile.Along with the difference of the various production technique before the polishing process can be divided into broad variety with polished tile, such as: pattern permeating tile, illusion-colour brick, micro-powder brick or the like.But no matter how complicated variation arranged, the manufacturing process flow process all is more or less the same, and perhaps accepts or rejects part technology, perhaps kinds of processes is mixed and uses.If hole, hole occur, being generally substandard product in the present polished tile, therefore, all is to adopt multiple mode to reduce the generation of hole in the existing polished tile production process.
And on the other hand, the decorative effect that lithotome had is commonly people and likes, take the course of its own aspect the wall decoration as the decorative effect that hole stone is showed, but natural cavity stone material price height, resource-constrained, and the artificial hole stone walling brick of producing can only adopt the mode of mould to make production at present, thereby its effect that shows nature inadequately, hole is had very much a rule, influences decorative effect.
Summary of the invention
The purpose of this invention is to provide a kind of porcelain brick with natural cavity stone decorative effect.
Another object of the present invention also is to provide a kind of preparation method who prepares the porcelain brick of above-mentioned natural cavity stone imitation.
The present invention realizes above-mentioned purpose by following technical solution: the porcelain brick of this natural cavity stone imitation, comprise the white material that existing porcelain brick is comprised, adding on the basis of white material has various inorganic color to be modulated into the powder of various color, the powder of various different colours mixes by a certain percentage unevenly can constitute various patterns and decorative pattern, it is characterized in that, also include the material that bubbles in this porcelain brick, the various raw material ratios of foaming material formula (siccative weight ratio) are: the ball clay class: 8~15 albite classes: 18~30 lithium feldspars: 30~45 Wingdales: 12~20 abrading block material: 0.5~3 burns talcum: 0~1; The Chemical Composition of its prescription is (weight ratio): table one
The prescription title SiO 2 Al 2O 3 Fe 2O 3 TiO 2 CaO MgO K 2O Na 2O Li 2O I.L
Material bubbles 58.0~62.4 122~14.6 0~0.6 0~05 8.2~9.7 1.7~2.5 1.4~1.9 3.8~4.4 0.35~0.7 8.1~9.6
All kinds of raw-material proportionings (siccative weight ratio) are in the described white material formula: the ball clay class: 24~28 high temperature sand classes: 15~25 albite classes: 35~50 potassium felspar sand classes: 6~17 burn talcum: 2~3; The Chemical Composition of its prescription is (weight ratio): table two
The prescription title SiO 2 Al 2O 3 Fe 2O 3 TiO 2 CaO MgO K 2O Na 2O Li 2O I.L
White material 67.5~70.0 18.2~20.0 0~0.6 0~0.5 0.2~0.7 0.5~1.0 1.4~1.9 3.8~4.4 - 4.0~4.8
Described abrading block material is for the polishing abrading block or make the starting material that polish abrading block, because the polishing slag is the waste residue in the polished tile course of processing, and two parts of scrap stock that abrading block that uses when comprising polishing and polished tile surface produce in grinding process; Because producing the composition of hole stone effect in the material that bubbles is the abrading block material, therefore described abrading block material can adopt the polishing slag to replace.
The invention also discloses a kind of method for preparing the porcelain brick of above-mentioned natural cavity stone imitation, it be existing porcelain brick production technique batching ball milling, the deironing of sieving, go into cylinder colour mixture, spraying drying, feed bin old, pulverize, at random batch mixing, the dry stamp of compression moulding, burn till on the basis of polishing, in the compression moulding process, adopt the grid pattern of natural-like stone lines; Being adopted as in batch mixing process at random simultaneously makes the stacked clearly flush system of this pattern lines in conjunction with the intermittent type cutting mode.
In above-mentioned manufacturing process, through the slurry that the ball milling wet-milling becomes, its slurry ball milling fineness is that 0.6g~0.8g 250 mesh sieves tail over; Slurry proportion: 1.7g/cm 3~1.75g/ Cm3Slurry moisture: 33%~35%; General porcelain brick has bed material and lining in producing, and bed material moisture is 6.6~7.0% after the drying operation, and the lining and the material moisture that bubbles are 5.0~5.6%; The proportioning of described foaming material in the porcelain brick lining is 2~15%, and the best is 3~5%.
The beneficial effect that the present invention adopts above-mentioned technical solution to reach is:
The present invention has developed the solution cavity effect that special foaming material formula makes product surface formation natural-like stone on the basis of the polished brick in porcelain character technological process of production of routine, and natural grid lines is imitated in design and improved " intermittently stacked flush system " cutting mode is planned the distribution and the trend of solution cavity.
In the present invention's prescription, various materials all have different separately effects: ball clay provides certain suspension property to guarantee not sedimentation of slurry; Albite, lithium feldspar, burning talcum all are used for reducing the prescription temperature makes visible vitreous luster in the hole; The lithium feldspar also can provide higher relatively high temperature viscosity to make bubble be difficult for breaking; Utilize abrading block material at low temperature sintering and rapid burning expansible characteristic to form bubble; And the CO that Wingdale at high temperature decomposes 2The effect that enlarges bubble is then arranged.
The present invention adopts the abrading block material as foam material, if adopt the polishing slag make the abrading block material that contains in the ceramic polished brick production process, then can utilization of waste material, and be beneficial to environmental protection;
The present invention adopts the carbonic acid gas that produces under the Wingdale high temperature to enlarge the effect of bubble-shaped cavitation stone; And the imitative natural grid lines of design and improved " intermittently stacked flush system " cutting mode, make product have natural cavity stone decorative effect true to nature, can be widely used in the wall decoration of top-grade building such as villa, hotel.
Description of drawings
Fig. 1 is a process flow diagram of the present invention.
Embodiment
The porcelain brick of natural cavity stone imitation of the present invention is made of white material and foaming material two portions, white material formula is identical with the other products of porcelain brick, add the powder that various inorganic color is modulated into various color on the basis of white material, the powder of various different colours mixes by a certain percentage unevenly can constitute various patterns and decorative pattern; The material that bubbles can form bubble not of uniform size in sintering procedure, thereby reaches special decorative effect.
Need to prove, it is waste residue in the polished tile course of processing that the abrading block material that uses in the material that bubbles also can adopt the polishing slag, the polishing cinder ladle is drawn together two parts of scrap stock that abrading block that when polishing use and polished tile surface produce in grinding process, the composition that helps to produce in the present invention hole stone effect is the abrading block material.Therefore, the abrading block material that uses among the present invention can use the polishing slag to replace, and the prescription content of this patent also should be not limited to the abrading block material, and should also comprise the foaming material that uses above substitute to make.
Be used for part starting material chemical ingredients of the present invention and see Table three.
Table three starting material Chemical Composition table
Material name SiO 2 Al 2O 3 Fe 2O 3 TiO 2 CaO MgO K 2O Na 2O Li 2O I.L Add up to
Ball clay 1# 53.92 30.59 0.73 0.29 0.14 0.16 0.8 0.22 - 12.82 99.67
Ball clay 2# 52.71 31.52 0.82 0.27 0.19 0.1 0.78 0.2 - 13.39 99.99
Albite 1# 71.81 17.36 0.19 0.04 0.24 0.14 0.28 8.96 - 0.84 99.87
Albite 2# 72.68 16.38 0.19 0.06 0.55 0.15 0.28 8.43 - 1.06 99.77
Albite 3# 73.03 16.23 0.18 0.06 0.28 0.13 0.47 8.32 - 1.05 99.74
Potassium felspar sand 1# 66.3 19.38 0.28 0.05 0.24 0.18 10.01 0.9 - 2.61 99.94
Potassium felspar sand 2# 76.6 14.29 0.26 0.04 0.14 0.16 4.35 1.04 - 2.84 99.72
Potassium felspar sand 3# 76.66 13.52 0.44 0.09 0.49 0.15 5.6 0.37 - 2.55 99.85
High temperature sand 1# 74.72 16.11 0.46 0.14 0.21 0.15 2.08 3.18 - 2.83 99.87
High temperature sand 2# 70.64 19.28 0.55 0.09 0.18 0.14 1.71 2.49 - 4.69 99.78
High temperature sand 3# 66.5 22.87 0.66 0.12 0.18 0.19 3.04 0.2 - 6.12 99.86
The lithium feldspar 73.61 17.62 0.34 0.11 0.39 0.17 2.07 3.31 1.38 0.92 99.92
The polishing slag 70.71 17.37 0.41 0.17 0.74 2.1 1.71 3.62 - 2.94 99.77
Burn talcum 64.68 1.36 0.15 0.04 2.77 29.73 0.07 0.1 - 0.84 99.73
Below providing concrete embodiment further specifies.The purpose of these embodiments is illustrative, and should not be construed as limitation of the present invention; Ball clay 1-2#, high temperature sand 1-3# albite 1-3#, potassium felspar sand 1-3# for various models all can be commercial, and it is selected for use can single model, or various model is mixed model and used and all can.
Example 1
White material formula (numbering CB-13):
Material name ratio (%)
Ball clay 1# 16
Ball clay 2# 9
Albite 1# 10
Albite 2# 17
Albite 3# 16
Potassium felspar sand 1# 3
Potassium felspar sand 2# 3
Potassium felspar sand 3# 7
High temperature sand 1# 9
High temperature sand 2# 5
High temperature sand 3# 3
Burn talcum 2
Add up to 100
Foaming material formula (numbering QP-01):
Material name ratio (%)
Lithium feldspar 38
Wingdale 17
Polishing slag 12
Albite 2 22
Ball clay 1# 10
Burn talcum 1
Add up to 100
More than the actual Chemical Composition of two prescriptions see Table four.
Table four prescription Chemical Composition table
The prescription title SiO 2 Al 2O 3 Fe 2O 3 TiO 2 CaO MgO K 2O Na 2O Li 2O I.L
White material 67.92 19.84 0.41 0.17 0.31 0.80 1.54 4.13 - 4.65
Material bubbles 60.4 13.24 0.28 0.14 8.59 2.02 1.43 4.1 0.43 8.89
Adopt after above the color matching technical process routinely to produce, use hole stone grid and 3# program (stacked flush system program at intermittence) in the process, specifically processing parameter is as follows:
(1), color matching:
A material: CB-13 (siccative) 100 grams+1.5 gram zirconium silicates
+ 0.1 gram true yellow+0.02 gram is orange for B material: CB-13 (siccative) 100 grams
Black material 0.01 gram of the orange+3# of C material: CB-13 (siccative) 100 grams+0.1 gram+apricot pink 0.05 gram
(2), lining proportioning:
1# pipe (1# groove) C material (red-black material) 10
2# pipe (2# groove) A material (white material) 30
3# manages (3# groove) QP-01 5
4# pipe (4# groove) B material (yellow material) 55
(3), lining moisture content: 5.0~5.6%
(4), lining fineness:
B material: 10~15% (80 mesh screen residues)
C material, A material, QP-01:20~25% (80 mesh screen residue)
(5), bed material proportioning: CB-13 material 100%
(6), bed material moisture content: 6.6~7.0%
(7), program: 3# program (intermittently stacked flush system)
(8), grid: hole stone grid
(9), compacting thickness: 13.6~14.0mm
Example 2
White material formula (numbering CB-13).
Foaming material formula (numbering QP-02):
Material name ratio (%)
Lithium feldspar 40
Wingdale 17
Polishing slag 5
Albite 2# 27
Ball clay 1# 10
Burn talcum 1
Add up to 100
Color matching and proportioning process parameter are as follows:
(1), color matching
Black material 0.04 gram of the beautiful Huang+3# of D material: CB-13 (siccative) 100 grams+0.6 gram+orange 0.15 gram
CB-04 material: CB-13 (siccative) 100 gram+zirconium silicates 2.0 grams
(2), lining proportioning:
1# pipe (1# groove) D material (dark brown colorant) 10
2# pipe (2# groove) D material 20%+CB-04 80% (white material) 25
3# pipe (3# groove) QP-02 material 5
4# pipe (4# groove) D material 70%+CB-04 30% (light brown material) 60
All other parameters are identical with " example 1 ".
It is existing porcelain brick production technique batching ball milling, the deironing of sieving, go into cylinder colour mixture, spraying drying, feed bin old, pulverize, at random batch mixing, the dry stamp of compression moulding, burn till on the basis of polishing, in the compression moulding process, adopt the grid pattern of natural-like stone lines; Being adopted as in batch mixing process at random simultaneously makes the stacked clearly flush system of this pattern lines in conjunction with the intermittent type cutting mode.Its first step adds wet-milling form slurry in the ball mill after need various starting material being pressed the accurate weighing of said ratio by technical process, and slurry ball milling fineness is that 0.6g~0.8g tails over (250 mesh sieve); Slurry proportion: 1.7g/cm 3~1.75g/cm 3Slurry moisture: 33%~35%.This slurry through slurry sieve, after the deironing, homogenizing, color matching spraying drying to the moisture that needs (bed material is 6.6~7.0%, and the lining and the material moisture that bubbles are 5.0~5.6%).
The powder of various different colours is according to the needs of design, in the cloth truck in the ratio of setting and blanking order blanking to the cloth grid and deliver to 800 * 800,600 * 600 adobes that press is pressed into to be needed.This process is beaten glomerocryst micro mist cloth, molding mode basically identical with traditional with the anti-of current trend, but in order to make product have the effect of natural cavity stone imitation more true to nature, we have improved traditional cutting mode.Traditional stacked flush system cutting mode is tiled on the distributing belt with making the powder continuous cloth of various different colours and a stacked one deck, sufficient batch mixing process is arranged at blanking during to hopper, the lines exquisiteness, and pattern is soft; The interval type cutting mode then is the at interval blanking of powder pulsed of various different colours, does not have overlappingly between powder on belt, need just can mix the formation pattern in hopper He on the grid, adopts the product lines of this cutting mode more extensive.With reference to the lines style of natural cavity stone, my company is improved to intermittently in conjunction with the advantage of two kinds of cutting modes that stacked flush system blanking reaches distinctive lines effect on stream.
Need to prove that in order to ensure the product hole distribution proportion suitable with natural cavity stone the proportioning of material in lining of bubbling is about 3~5%, in order to make special product effect, the proportioning of the material that bubbles can be increased to 15% even 18% or higher.In order to reach the effect of hole distribution preferably, it is crucial adopting proportion, moisture and the slurry ball milling fineness of suitable slurry, lining and the material that bubbles, and through enforcement, above-mentioned scope of the present invention is ideal.
As Fig. 1, technical process of the present invention is described below:
Raw material is checked and accepted the examination that the into raw-material examination of factory comprises sand, stone flour, mud and various chemical industry material, colorant.Factory has formulated various standard for acceptance and by a collection of professional's operative norm, has guaranteed to use high-quality raw material various starting material according to different use propertieies, requirement.
The batching ball milling is formulated various raw-material producting proportions according to the test-results of person skilled, and prepare burden according to this proportioning, by conveying belt various starting material are sent into the 40T ball mill then, add again that the roating sphere grinding machine becomes the mud slurry with the starting material ball milling after the entry.This process approximately needed do not wait in 12~18 hours, and the time is depended on the fineness of mud slurry, and technic index requires to be controlled at 250 mesh screen residues less than 1.0% usually.Slurry after the ball milling carries out the stability of homogenizing to guarantee to produce by the underground stock tank that pipeline flow into hundreds of tons of capacity.
It is that starting material thick excessively in the production process, impurity and various foreign matter are sifted out that the deironing of sieving is sieved; Deironing is by bar magnet the irony in the mud slurry to be removed.Because these things will have very large detrimentally affect to quality product, altogether need be in the production process through three deironing of sieving.
The mud slurry of going into cylinder colour mixture front is white, has the different colours of various needs in order to make product, need add the different colorants of measuring in the mud slurry.The control of colorant add-on need constantly test be next definite by the professional and technical personnel.In order to ensure the homogeneity of colorant, colorant also needs fully to mix by high-power stirrer after adding.
The slurry of spraying drying colour mixture is through carrying out spraying drying after the deironing once more.Spraying drying is the process that the mud slurry is dried to powder.Principle is: mud slurry is dispersed into vaporific by spray gun, the warm air that comes with convection current carries out heat exchange afterwards, the moisture evaporation during vaporific mud is starched, and other ceramic raw material has just become powder.Need emphasis to control the size of vaporific mud slurry and the temperature of warm air in this process, because they have determined the grain composition and the moisture of powder respectively.
Feed bin is old because varying in size of vaporific mud slurry causes the difference of heat exchange, finally causes the moisture of powder to have any different.After powder after the spraying drying is delivered to filler bin by conveying belt, even in order to make moisture, powder need be placed 24 hours at least usually.Meanwhile, owing to having suitable temperature and moisture, the microorganism in the powder also will multiply fast and will producing favorable influence to the processability of powder.Therefore, this process is called as old.
Pulverizing different products has different requirements for the fineness of powder, and common pattern permeating tile, illusion-colour etc. do not need to pulverize, and can directly use spraying material.Micro-powder brick then needs powder is pulverized.Crushing process promptly is the process of powder being processed by specific equipment (sander or powder beater), can control the fineness of powder by regulating motor speed.
Batch mixing carries out at random by the powder vehicle device to the different colours powder that batch mixing forms the various pattern of brick face at random.Different ratios between different powder cars, cutting mode, blanking order, the powder can form various pattern in the batch mixing process.Powder behind the batch mixing is transported to the voltage supply of press die cavity by powder car parts " grid " and makes type.Most on the market product innovation all is to produce by the different processes of batch mixing at random at present.
Being molded over having shades of colour and having formed the powder of pattern through batch mixing at random of producing before this operation must be by the shape of press compacting could formation brick.The process of complexity such as the exhaust of this process by hydraulic press, compacting is discharged the moisture between powder and powder is combined closely and becomes to have the work in-process of certain intensity.Can adopt the press of the different tonnages of 2800T~7200T according to varying in size of product specification.
Dry can press-molding in order to ensure powder, spray-dired powder remains on 6.0~8.0% moisture usually, these water need by the oven dry of roller bed type dry kiln to the moisture 1.0% below to guarantee descending operation to burn till fast.Adobe in dry kiln successively the air by low temperature and high relative humidity, high temperature low humidity carry out heat exchange and exchange of moisture process, can reach processing requirement after about 40~60 minutes.
Stamp is for pattern permeating tile, and its pattern mainly forms by stamp.But the soluble salt of various color developments and water, the mixed fancy glaze that makes of penetration-assisting agent, the scraper with the flower machine makes fancy glaze be printed in the adobe by the colored net that specific pattern is arranged again, and these fancy glazes form decorative pattern through firing the back.
Burning till adobe moves in the roller bed type calcining kiln, temperature rises to 1200 ℃ from room temperature and reduces to room temperature again, series of physical, chemical transformation such as moisture evaporation, decomposition, oxidation, fusion, crystallization have taken place in the process, have finally become irreversible ceramic product.
Polishing has higher glossiness in order to make product, also need to product surface scrape, cut, post-production such as mill handles.Simultaneously, meet the requirement of relevant criterion, need the product edging is handled in order to guarantee product size.
Classification is carried out classification, color separation according to relevant criterion (national standard, enterprise's inner quality standard etc.) to product, and different grades, not homochromy number product are separately deposited.
Packing is packed, is identified and put in storage product according to the demand of product protection.
More than the preparation method of hole provided by the present invention stone porcelain brick is described in detail, used specific case herein principle of the present invention and embodiment are set forth, the explanation of above embodiment just is used for helping to understand method of the present invention and core concept thereof; Simultaneously, for the general technology person of this area, according to thought of the present invention, the part that all can change in specific embodiments and applications, in sum, this description should not be construed as limitation of the present invention.

Claims (8)

1, a kind of porcelain brick of natural cavity stone imitation, comprise the white material that existing porcelain brick is comprised, adding on the basis of white material has various inorganic color to be modulated into the powder of various color, the powder of various different colours mixes by a certain percentage unevenly can constitute various patterns and decorative pattern, it is characterized in that, also include the material that bubbles in this porcelain brick, the various raw material ratios of foaming material formula (siccative weight ratio) are: the ball clay class: 8~15 albite classes: 18~30 lithium feldspars: 30~45 Wingdales: 12~20 abrading block material: 0.3~3 burns talcum: 0~1; The Chemical Composition of its prescription is (weight ratio):
The prescription title SiO 2 Al 2O 3 Fe 2O 3 TiO 2 CaO MgO K 2O Na 2O Li 2O I.L Material bubbles 58.0~62.4 12.2~14.6 0~0.6 0~0.5 82~9.7 1.7~23 1.4~1.9 3.8~4.4 0.35~0.7 8.1~9.6
2, the porcelain brick of natural cavity stone imitation according to claim 1, it is characterized in that all kinds of raw-material proportionings (siccative weight ratio) are in the described white material formula: the ball clay class: 24~28 high temperature sand classes: 15~25 albite classes: 35~50 potassium felspar sand classes: 6~17 burn talcum: 2~3; The Chemical Composition of its prescription is (weight ratio):
The prescription title SiO 2 Al 2O 3 Fe 2O 3 TiO 2 CaO MgO K 2O Na 2O Li 2O I.L White material 67.5~70.0 18.2~20.0 0~0.6 0~0.5 0.2~0.7 0.5~1.0 1.4~1.9 3.8~4.4 - 4.0~4.8
3, the porcelain brick of natural cavity stone imitation according to claim 1, it is characterized in that, described abrading block material adopts the polishing slag that contains abrading block material composition, this polishing slag is the waste residue in the polished tile course of processing, two parts of scrap stock that abrading block that uses when comprising polishing and polished tile surface produce in grinding process, its proportioning is (weight ratio) 3-15.
4, a kind of method for preparing the porcelain brick of each described natural cavity stone imitation of claim 1-3, it is characterized in that, it be existing porcelain brick production technique batching ball milling, the deironing of sieving, go into cylinder colour mixture, spraying drying, feed bin old, pulverize, at random batch mixing, the dry stamp of compression moulding, burn till on the basis of polishing, in the compression moulding process, adopt the grid pattern of natural-like stone lines; Adopting in batch mixing process at random simultaneously makes the stacked clearly flush system of this pattern lines in conjunction with the intermittent type cutting mode.
5, the porcelain brick preparation method of natural cavity stone imitation according to claim 4 is characterized in that, through the slurry that the ball milling wet-milling becomes, its slurry ball milling fineness is that 0.6g~0.8g 250 mesh sieves tail over; Slurry proportion: 1.7g/cm 3~1.75g/cm 3Slurry moisture: 33%~35%.
6, the porcelain brick preparation method of natural cavity stone imitation according to claim 4 is characterized in that, the bed material moisture of adobe after the drying operation is 6.6~7.0%, and the lining of porcelain brick and the material moisture that bubbles are 5.0~5.6%.
According to the porcelain brick preparation method of claim 4 or 6 described natural cavity stone imitations, it is characterized in that 7, the proportioning of described foaming material in the lining of porcelain brick is 2~15%.
8, the porcelain brick preparation method of natural cavity stone imitation according to claim 7 is characterized in that, the proportioning of described foaming material in the lining of porcelain brick is 3-5%.
CNB2007100263238A 2007-01-10 2007-01-10 Natural travertine-imitated ceramic brick and making method Expired - Fee Related CN100439280C (en)