CN104761663A - Recovered modified PVA gel and preparation and application methods thereof - Google Patents

Recovered modified PVA gel and preparation and application methods thereof Download PDF

Info

Publication number
CN104761663A
CN104761663A CN201410746326.9A CN201410746326A CN104761663A CN 104761663 A CN104761663 A CN 104761663A CN 201410746326 A CN201410746326 A CN 201410746326A CN 104761663 A CN104761663 A CN 104761663A
Authority
CN
China
Prior art keywords
reactor
pva
temperature
recovered
preparation
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
CN201410746326.9A
Other languages
Chinese (zh)
Inventor
田培善
林源杰
吕福菊
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
West (wuxi) Biotechnology Co Ltd
Original Assignee
West (wuxi) Biotechnology Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by West (wuxi) Biotechnology Co Ltd filed Critical West (wuxi) Biotechnology Co Ltd
Priority to CN201410746326.9A priority Critical patent/CN104761663A/en
Publication of CN104761663A publication Critical patent/CN104761663A/en
Withdrawn legal-status Critical Current

Abstract

The invention discloses a recovered modified PVA gel and preparation and application methods thereof, belonging to field of chemistry. A composite particle of carboxy methyl starch and recovered PVA which can be used for sizing is prepared by crushing a recovered PVA film, modifying the recovered PVA film with chemical reagents like sodium hydroxide, hydrogen peroxide and ferrous chloride, and subjecting modified PVA gel and carboxy methyl starch to mixing with stirring, granulation, drying, blanking, cooling and crushing. The invention discloses a recycling method for the PVA film. Modified PVA is easily biodegradable, so environmental pressure is reduced and sizing cost is lowered down.

Description

一种回收改性PVA胶体及其制备和应用方法A kind of recovery modified PVA colloid and its preparation and application method

技术领域 technical field

本发明涉及化学领域,具体为一种回收改性PVA胶体及其制备和应用方法。 The invention relates to the field of chemistry, in particular to a recovery modified PVA colloid and a preparation and application method thereof.

背景技术 Background technique

纺织工业存在的污染主要是有湿加工整理排放的污水造成的。这些湿加工整理包括织物的退浆、煮练、漂白、印花及后整理等。其中退浆造成的污染超过50%,其根源就就是浆纱过程中所用的浆料。纺织上浆的主体浆料是变性淀粉、聚乙烯醇(PVA)和聚丙烯酸类浆料。含有PVA废水的BOD5/COD比值为0.02-0.05,在水体中很难生物降解,对水环境造成了很大压力。因此出口到欧盟的服装常常要求使用可循环使用的PVA膜材料,并由服装供应商负责收回使用,因此如何提高回收PVA膜材料并实现循环使用是本行业的一大技术难题。 The pollution in the textile industry is mainly caused by the sewage discharged from wet processing. These wet processing and finishing include desizing, scouring, bleaching, printing and finishing of fabrics. Among them, the pollution caused by desizing exceeds 50%, and its root cause is exactly the size used in the sizing process. The main size of textile sizing is modified starch, polyvinyl alcohol (PVA) and polyacrylic size. The BOD5/COD ratio of PVA-containing wastewater is 0.02-0.05, which is difficult to biodegrade in water bodies and causes great pressure on the water environment. Therefore, garments exported to the EU often require the use of recyclable PVA film materials, and the garment suppliers are responsible for recycling. Therefore, how to improve the recovery of PVA film materials and realize recycling is a major technical problem in this industry.

发明内容 Contents of the invention

鉴于以上所述现有技术的缺点,本发明对回收的PVA膜进行改性处理,然后再与淀粉复合烘干,做成含PVA的复合颗粒材料,作为纺织上浆的纤维粘合剂,从而实现了PVA膜的循环使用,并节省了上浆成本。 In view of the above-mentioned shortcoming of the prior art, the present invention carries out modification treatment to the reclaimed PVA film, then combines and dries with starch, makes the composite granular material containing PVA, as the fiber binder of textile sizing, thereby realizes It improves the recycling of PVA film and saves the cost of sizing.

回收PVA膜的改性制备方法,包括如下步骤: The modified preparation method of reclaiming PVA film comprises the steps:

(1)将回收的PVA膜进行粉碎处理; (1) Crushing the recovered PVA film;

(2)向2000L的反应釜中加入粉碎处理的200kgPVA膜,然后在向反应釜中加入700kg的水; (2) Add 200kg of pulverized PVA film to the 2000L reactor, and then add 700kg of water to the reactor;

(3)搅拌反应釜中的混合溶液,在搅拌的同时加入10-20kg的氢氧化钠和质量浓度为50%的双氧水; (3) Stir the mixed solution in the reactor, add 10-20kg of sodium hydroxide and hydrogen peroxide with a mass concentration of 50% while stirring;

(4)加热反应釜至反应釜内混合溶液温度为50-60℃时,滴加10-15kg质量浓度为9%氯化亚铁溶液; (4) Heat the reactor until the temperature of the mixed solution in the reactor is 50-60°C, add 10-15kg of ferrous chloride solution with a mass concentration of 9% dropwise;

(5)加热反应釜至反应釜内混合溶液温度为60-70℃,保温4小时,然后再加热反应釜至反应釜内混合溶液温度为90-100℃,保温30分钟; (5) Heat the reactor until the temperature of the mixed solution in the reactor is 60-70°C, keep it warm for 4 hours, then heat the reactor until the temperature of the mixed solution in the reactor is 90-100°C, keep it warm for 30 minutes;

(6)自然冷却反应釜温度至不大于40℃时,滴加质量浓度为30%的稀硫酸直至反应釜中溶液的PH值为6-8,制得回收改性PVA胶体。 (6) When the temperature of the reaction kettle is naturally cooled to no more than 40°C, dilute sulfuric acid with a mass concentration of 30% is added dropwise until the pH value of the solution in the reaction kettle is 6-8, and the recovered modified PVA colloid is obtained.

优选的,步骤(1)中所诉的粉碎处理采用单轴撕碎机粉碎,所述单轴撕碎机的主轴转速为70-80 转/分。 Preferably, the pulverization process described in step (1) is pulverized by a single-shaft shredder, and the spindle speed of the single-shaft shredder is 70-80 rpm.

优选的,步骤(1)中所诉的粉碎处理的颗粒直径不大于40mm。 Preferably, the particle diameter of the pulverized particles in step (1) is not greater than 40mm.

优选的,步骤(4)中所诉的滴加氯化亚铁溶液,在25-30分钟内滴加完成。 Preferably, the dropwise addition of ferrous chloride solution described in step (4) is completed dropwise within 25-30 minutes.

通过上述方法制备的回收改性PVA胶体,外观淡黄色粘稠液体,含固量23%-24%,粘度10-20 mPa.S。 The recovered modified PVA colloid prepared by the above method has a light yellow viscous liquid appearance, a solid content of 23%-24%, and a viscosity of 10-20 mPa.S.

通过上述方法制备的回收改性PVA胶体的应用方法,包括如下步骤: The application method of the reclaimed modified PVA colloid prepared by said method comprises the steps:

(a)将50-55kg的权利要求5项所述的回收改性PVA胶体与110-126kg的淀粉搅拌混合; (a) stirring and mixing 50-55kg of the recovered modified PVA colloid described in claim 5 with 110-126kg of starch;

(b)将步骤(a)所述的搅拌混合物进行造粒处理; (b) granulating the stirred mixture described in step (a);

(c)将造粒处理后的颗粒进行干燥处理; (c) Drying the granulated granules;

(d)将干燥处理后的颗粒,出料、冷却并粉碎。 (d) Discharging, cooling and pulverizing the dried granules.

优选的,步骤(a)所述的搅拌混合,时间为5-10分钟,步骤(b)所述的造粒处理,时间为20-50分钟,步骤(c)所述的干燥处理,温度为80-95℃,步骤(d)所述的出料,温度为80-82℃。 Preferably, the mixing time in step (a) is 5-10 minutes, the granulation treatment in step (b) is 20-50 minutes, and the drying treatment in step (c) is at a temperature of 80-95°C, the temperature of the discharge described in step (d) is 80-82°C.

优选的,步骤(a)所述的淀粉为羧甲基淀粉。 Preferably, the starch described in step (a) is carboxymethyl starch.

本发明提供了一种回收改性PVA胶体及其制备和应用方法,在回收PVA膜改性处理过程中使用了双氧水、氯化亚铁、氢氧化钠等化学试剂,双氧水在亚铁离子的催化作用下能够将PVA上的羟基氧化成羰基。 The invention provides a recovery modified PVA colloid and its preparation and application method. Chemical reagents such as hydrogen peroxide, ferrous chloride and sodium hydroxide are used in the process of recovery of PVA film modification. Under the action, the hydroxyl group on PVA can be oxidized to carbonyl group.

为了保持PVA的本身特性,双氧水用量的确定以氧化PVA的分子量为依据,从而严格控制其氧化程度,让PVA分子链断裂程度适中,使聚合度控制在1400-1700之间。 In order to maintain the inherent characteristics of PVA, the amount of hydrogen peroxide is determined based on the molecular weight of oxidized PVA, so as to strictly control its oxidation degree, so that the degree of PVA molecular chain breakage is moderate, and the degree of polymerization is controlled between 1400-1700.

在改性反应过程中通过显色法定时检测反应过程中PVA的羟基含量,从而确定了氧化所需要的时间及反应程度。 During the modification reaction process, the hydroxyl content of PVA in the reaction process is detected regularly by colorimetric method, so as to determine the time required for oxidation and the degree of reaction.

由于H2O2的分解温度为80℃,因此反应温度不能太高,所以在步骤(5)中选择的反应温度为60-70℃。 Since the decomposition temperature of H 2 O 2 is 80°C, the reaction temperature cannot be too high, so the reaction temperature selected in step (5) is 60-70°C.

具体实施方式 Detailed ways

实施例1 Example 1

回收PVA膜的改性制备,包括如下步骤: The modified preparation of recovery PVA membrane comprises the steps:

(1)将回收的PVA膜用单轴撕碎机粉碎,单轴撕碎机的主轴转速为70-80 转/分,粉碎后的粉末用直径为40mm的过滤筛进行过滤处理; (1) Pulverize the recovered PVA film with a single-shaft shredder, the spindle speed of the single-shaft shredder is 70-80 rpm, and the pulverized powder is filtered with a filter screen with a diameter of 40mm;

(2)向2000L的反应釜中加入粉碎处理的200kgPVA膜,然后在向反应釜中加入700kg的水; (2) Add 200kg of pulverized PVA film to the 2000L reactor, and then add 700kg of water to the reactor;

(3)搅拌反应釜中的混合溶液,在搅拌的同时加入10-20kg的氢氧化钠和质量浓度为50%的双氧水; (3) Stir the mixed solution in the reactor, add 10-20kg of sodium hydroxide and hydrogen peroxide with a mass concentration of 50% while stirring;

(4)加热反应釜至反应釜内混合溶液温度为50-60℃时,在25-30分钟内滴加完10-15kg质量浓度为9%氯化亚铁溶液; (4) Heat the reactor until the temperature of the mixed solution in the reactor is 50-60°C, and drop 10-15kg of 9% ferrous chloride solution within 25-30 minutes;

(5)加热反应釜至反应釜内混合溶液温度为60-70℃,保温4小时,然后再加热反应釜至反应釜内混合溶液温度为90-100℃,保温30分钟; (5) Heat the reactor until the temperature of the mixed solution in the reactor is 60-70°C, keep it warm for 4 hours, then heat the reactor until the temperature of the mixed solution in the reactor is 90-100°C, keep it warm for 30 minutes;

(6)自然冷却反应釜温度至不大于40℃时,滴加质量浓度为30%的稀硫酸直至反应釜中溶液的PH值为6-8,制得回收PVA胶体。 (6) When the temperature of the reaction kettle is naturally cooled to no more than 40°C, dilute sulfuric acid with a mass concentration of 30% is added dropwise until the pH value of the solution in the reaction kettle is 6-8 to obtain recovered PVA colloid.

改性处理后的回收PVA溶液,外观淡黄色粘稠液体,含固量23%-24%,粘度10-20 mPa.S。 The recovered PVA solution after modification treatment is a light yellow viscous liquid with a solid content of 23%-24% and a viscosity of 10-20 mPa.S.

回收PVA胶体的应用方法,包括如下步骤: The application method of reclaiming PVA colloid may further comprise the steps:

(a)将50-55kg的回收改性PVA胶体与110-126kg的羧甲基淀粉搅拌混合,搅拌5-10分钟; (a) Stir and mix 50-55kg of recovered modified PVA colloid and 110-126kg of carboxymethyl starch, and stir for 5-10 minutes;

(b)将步骤(a)所述的搅拌混合物进行造粒处理,造粒时间为20-50分钟; (b) granulating the stirred mixture described in step (a), and the granulation time is 20-50 minutes;

(c)将造粒处理后的颗粒,在80-95℃进行干燥处理; (c) Drying the granulated granules at 80-95°C;

(d)将干燥处理后的颗粒,出料、冷却并粉碎。 (d) Discharging, cooling and pulverizing the dried granules.

本发明回收改性制备PVA胶体的生物降解性能的测试。 The invention recovers and modifies and prepares the biodegradability test of the PVA colloid.

取本发明回收改性制备PVA胶体样品,市场上购置的PVA-1799(颗粒)、PVA-0588(颗粒),分别用蒸馏水配制成1 g/L的试验水样,进行对比试验,分别检测三种溶液的BOD5和COD。 Take the PVA colloid sample prepared by the recovery and modification of the present invention, PVA-1799 (granule) and PVA-0588 (granule) purchased on the market are prepared into 1 g/L test water samples with distilled water respectively, and a comparative test is carried out to detect three BOD5 and COD of the solution.

试验水样(1.0g/L)Test water sample (1.0g/L) BOD5BOD5 CODCOD BOD5/BODBOD5/BOD 回收改性制备PVA胶体Preparation of PVA Colloid by Recycling and Modification 8888 12981298 0.068 0.068 PVA-1799PVA-1799 2929 13181318 0.022 0.022 PVA-0588PVA-0588 4343 12641264 0.034 0.034

结果表明回收改性PVA胶体的BOD5/BOD比值提高了一倍以上。 The results showed that the BOD5/BOD ratio of recovered modified PVA colloid was more than doubled.

浆纱试验 Sizing test

试验品种: Test species:

涤棉纱线在整浆联合试验机上试验T65/C35  45支、总经320根(8层)。前筘幅20 CM试验覆盖系数40%相当于双浆槽做经密。常用调浆,浆纱机速度20米/min。单浆槽,双浸双压。浆纱烘干温度100-105℃。 T65/C35 45 counts and 320 total warp (8 layers) of polyester-cotton yarns were tested on the pulping joint testing machine. The test coverage factor of 40% with a front reed width of 20 CM is equivalent to the warp density of double pulp tanks. Commonly used for sizing, the speed of the sizing machine is 20 m/min. Single slurry tank, double dipping and double pressing. The sizing drying temperature is 100-105°C.

试验浆纱配方如下 The test sizing formula is as follows

方案plan PVA-1799PVA-1799 氧化淀粉Oxidized starch 浆纱蜡片Sizing Wax 回收改性PVA与羧甲基淀粉的复合颗粒Recovery of Composite Granules of Modified PVA and Carboxymethyl Starch 设定含固量Set solid content AA 2020 4747 1.51.5  the 13%13% BB  the  the 1.51.5 6767 13%13%

浆纱质量指标如下: Sizing quality indicators are as follows:

项目project 回潮率Moisture regain 强力(CN)Strong (CN) 伸长elongation 耐磨次数Wear times 退浆率Desizing rate 毛羽数(3mm)Hairiness (3mm) 方案AOption A 2.62%2.62% 378.4378.4 8.80%8.80% 45.345.3 13.46%13.46% 1862.01862.0 方案BOption B 2.61%2.61% 381.2381.2 8.94%8.94% 46.846.8 13.21%13.21% 1639.51639.5

方案B的浆纱质量全面优于方案A的指标。 The sizing quality of scheme B is better than that of scheme A in all respects.

挥发份、粘度稳定性的检测方法参照纺织常用变性淀粉浆料质量行业标准(2000版,试行)。 The detection methods of volatile matter and viscosity stability refer to the industry standard for the quality of modified starch sizing commonly used in textiles (version 2000, trial implementation).

粘度检测采用NDJ-79型旋转式粘度计检测粘度,参照GB12098-89的方法进行。 Viscosity detection adopts NDJ-79 rotary viscometer to detect viscosity, referring to the method of GB12098-89.

Claims (8)

1.一种回收PVA胶体的改性制备方法,其特征在于,包括如下步骤: 1. a modified preparation method of reclaiming PVA colloid, is characterized in that, comprises the steps: (1)将回收的PVA膜进行粉碎处理; (1) Crushing the recovered PVA film; (2)向2000L的反应釜中加入粉碎处理的200kgPVA膜颗粒,然后在向反应釜中加入700kg的水; (2) Add 200kg of pulverized PVA film particles to the 2000L reactor, and then add 700kg of water to the reactor; (3)搅拌反应釜中的混合溶液,在搅拌的同时加入10-20kg的氢氧化钠和质量浓度为50%的双氧水; (3) Stir the mixed solution in the reactor, add 10-20kg of sodium hydroxide and hydrogen peroxide with a mass concentration of 50% while stirring; (4)加热反应釜至反应釜内混合溶液温度为50-60℃时,滴加10-15kg质量浓度为9%氯化亚铁溶液; (4) Heat the reactor until the temperature of the mixed solution in the reactor is 50-60°C, add 10-15kg of ferrous chloride solution with a mass concentration of 9% dropwise; (5)加热反应釜至反应釜内混合溶液温度为60-70℃,保温4小时,然后再加热反应釜至反应釜内混合溶液温度为90-100℃,保温30分钟; (5) Heat the reactor until the temperature of the mixed solution in the reactor is 60-70°C, keep it warm for 4 hours, then heat the reactor until the temperature of the mixed solution in the reactor is 90-100°C, keep it warm for 30 minutes; (6)自然冷却反应釜温度至不大于40℃时,滴加质量浓度为30%的稀硫酸直至反应釜中溶液的PH值为6-8,制得回收PVA胶体。 (6) When the temperature of the reaction kettle is naturally cooled to no more than 40°C, dilute sulfuric acid with a mass concentration of 30% is added dropwise until the pH value of the solution in the reaction kettle is 6-8 to obtain recovered PVA colloid. 2.根据权利要求1所述的改性制备方法,其特征在于,步骤(1)中所诉的粉碎处理采用单轴撕碎机粉碎,所述单轴撕碎机的主轴转速为70-80 RPM/分。 2. The modification preparation method according to claim 1, characterized in that, the crushing treatment in step (1) is crushed by a single-shaft shredder, and the spindle speed of the single-shaft shredder is 70-80 RPM/min. 3.根据权利要求1所述的改性制备方法,其特征在于,步骤(1)中所诉的粉碎处理的颗粒直径不大于40mm。 3. The modification preparation method according to claim 1, characterized in that the particle diameter of the pulverized particles in step (1) is not greater than 40mm. 4.根据权利要求1所述的改性制备方法,其特征在于,步骤(4)中所诉的滴加氯化亚铁溶液,在25-30分钟内滴加完成。 4. The modification preparation method according to claim 1, characterized in that the dropwise addition of ferrous chloride solution in step (4) is completed within 25-30 minutes. 5.一种回收改性PVA胶体,其特征在于,通过权利要求1-4任一项所述的方法制备,外观淡黄色粘稠液体,含固量23%-24%,粘度10-20 mPa.S。 5. A reclaimed modified PVA colloid, characterized in that, prepared by the method described in any one of claims 1-4, the appearance is light yellow viscous liquid, with a solid content of 23%-24%, and a viscosity of 10-20 mPa .S. 6.一种回收PVA胶体的应用方法,其特征在于,包括如下步骤: 6. an application method of reclaiming PVA colloid, is characterized in that, comprises the steps: (a)将50-55kg的权利要求5项所述的回收改性PVA胶体与110-126kg的淀粉搅拌混合; (a) stirring and mixing 50-55kg of the recovered modified PVA colloid described in claim 5 with 110-126kg of starch; (b)将步骤(a)所述的搅拌混合物进行造粒处理; (b) granulating the stirred mixture described in step (a); (c)将造粒处理后的颗粒进行干燥处理; (c) Drying the granulated granules; (d)将干燥处理后的颗粒,出料、冷却并粉碎。 (d) Discharging, cooling and pulverizing the dried granules. 7.根据权利要求6所述的应用方法,其特征在于,步骤(a)所述的搅拌混合,时间为5-10分钟,步骤(b)所述的造粒处理,时间为20-50分钟,步骤(c)所述的干燥处理,温度为80-95℃,步骤(d)所述的出料,温度为80-82℃。 7. The application method according to claim 6, characterized in that the stirring and mixing in step (a) takes 5-10 minutes, and the granulation treatment in step (b) takes 20-50 minutes , the drying treatment described in step (c), the temperature is 80-95°C, and the discharge described in step (d), the temperature is 80-82°C. 8.根据权利要求6所述的应用方法,其特征在于, 步骤(a)所述的淀粉为羧甲基淀粉。 8. The application method according to claim 6, characterized in that, the starch described in step (a) is carboxymethyl starch.
CN201410746326.9A 2014-12-09 2014-12-09 Recovered modified PVA gel and preparation and application methods thereof Withdrawn CN104761663A (en)