CN106930121A - Plain color umbrella cloth color-changing printing technique - Google Patents
Plain color umbrella cloth color-changing printing technique Download PDFInfo
- Publication number
- CN106930121A CN106930121A CN201710166650.7A CN201710166650A CN106930121A CN 106930121 A CN106930121 A CN 106930121A CN 201710166650 A CN201710166650 A CN 201710166650A CN 106930121 A CN106930121 A CN 106930121A
- Authority
- CN
- China
- Prior art keywords
- color
- glue
- sizing
- stamp
- yards
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The present invention relates to a kind of plain color umbrella cloth color-changing printing technique, it be by plain color A grades of fabric it is dyed → treatment of preparation → gluing → stamp → washing → centre sizing → second glue spreading → finished product shaping process of sizing can be prepared by color-changing printing umbrella cloth finished product.The umbrella cloth prepared by color-changing printing technique of the invention can't see flower pattern under dry state, and flower pattern is showed under hygrometric state, show unique characteristics so that product possesses the good market competitiveness;In addition, special printing technology of the invention is standardized production, technological process temperature so that the uniformity of product is very strong, obtained excellent product quality, stable performance, with more than 3 years service life.
Description
Technical field
The present invention relates to a kind of printing technology of umbrella cloth, a kind of plain color umbrella cloth color-changing printing technique is particularly related to.
Background technology
Umbrella is commodity extremely common in living, and umbrella cloth is the main member of umbrella.Rain common in the market
Although the umbrella cloth of umbrella is printed with aesthetic pattern miscellaneous, but all lacks characteristic so that the competitiveness of product is not strong.
The content of the invention
The present invention provides a kind of plain color umbrella cloth color-changing printing technique, does not have spy with overcome existing umbrella cloth to exist
Color, the not strong problem of competitiveness.
The present invention is adopted the following technical scheme that:
Plain color umbrella cloth color-changing printing technique, including the following step for carrying out successively:
A. dye:Plain color A grades of fabric is dyed into required base color;
B. preparation sizing:Door width on request(That is cloth cover width)Carry out preparing sizing, sky determines place and is unable to water-sprinkling;
C. a gluing:By PUR, methyl esters with 20~23:4 ratio is mixed to prepare with glue;First on the fabric of preparation sizing
Coating primer, is coated with glue;Primer use viscosity for 17000~18000 PUR, speed be 55~62 yards/minute, dry
It is dry;
D. stamp:Former paste is made using sodium alginate, it is 4500~5500 that the water repellent of addition 6~8% by weight proportion is tuned into viscosity
Printing paste;Stamp is carried out using the printing paste by printing machine, printing machine speed is 35~40 yards/minute, and stamp is by temperature
The drying room spent for 130~140 DEG C is dried;
E. wash:Washed by rinsing machine in machine 2~3 hours under stamp, glue surface is upward during washing;Washing process is,
A. the first groove puts flowing cool water;B. second adds 1.7~2.3g/L of sodium hydrosulfite, 0.8~1.2g/L of caustic soda to N grooves, and temperature is 80
~85 DEG C, each groove of this step must change water once during 4000 yards or so of cloth cover of washing, and speed is 40~45 yards/minute;
C. N+1 grooves heating degree is 55~60 DEG C of warm water, and N+2 grooves add flowing cool water;When d. drying, cloth cover keeps 70~80%
Aridity;
F. sizing in the middle of:Door width is allocated on request, and temperature is 150 DEG C ± 3 DEG C, yard/minute of speed 63~70;
G. second glue spreading:Coating is that raw material preparation viscosity is 9200~11000 with glue with PUR and methyl esters;
H. finished product sizing:Door width is allocated on request, and temperature is 120~130 DEG C, and speed is 40~48 yards/minute, and sky determines place can not
Water-sprinkling;It is finished product after finished product sizing.
Further, plain color color-changing printing umbrella cloth is preferably produced by following techniques, and the technique by carrying out successively
Following step constitute:
A. dye:Plain color A grades of fabric is dyed into required base color;
B. preparation sizing:Door width applies setting agent to carry out preparing sizing at the place of specifying on request, and sky determines place and is unable to water-sprinkling, and sky is fixed
It refer to the position for not applying setting agent;
C. a gluing:By PUR(It is commonly called as virgin rubber, film), methyl esters is with 21:4 ratio is mixed to prepare with glue;First in preparation
Primer is coated with the fabric of sizing, is coated with glue;Primer use viscosity for 17000~18000 PUR, dark color apply elargol
Shi Caiyong coloring agents are 60 yards/minute as primer, speed, need drying;It is required that glue can not front thoroughly, glue surface is uniform;200 yards of start
Inside need check cloth cover whether seep through;
D. stamp:Former paste is made using sodium alginate, the water repellent that 7% is added by weight proportion is tuned into the printing paste that viscosity is 5000;
Stamp is carried out using the printing paste by printing machine, printing machine speed is 35~40 yards/minute, stamp by temperature be 130~
140 DEG C of drying room is dried;Leftover of bolt of cloth positive and negative will identify clear, and stamp cannot pass through the fabric guide roll not rotated, spiral shell into and out of cloth
Line spread roller can not open friction glue surface, and stamp arc will swathe one layer of woven dacron to reduce frictional heating, start shooting for a long time
When need appropriate to shut down cooling;
E. wash:Washed by rinsing machine in machine 2~3 hours under stamp, glue surface is upward during washing;Washing process is,
A. the first groove puts flowing cool water;B. second and third, four, five grooves add sodium hydrosulfite 2g/L, caustic soda 1g/L, temperature is 80~85 DEG C, washing
Each groove of this step must change water once during 4000 yards or so of cloth cover, and speed is 40~45 yards/minute;C. the 6th groove heating
The warm water for 55~60 DEG C is spent, the 7th groove adds flowing cool water;When d. drying, cloth cover keeps 70~80% aridity;
F. sizing in the middle of:Door width is allocated on request(Allocate i.e. cloth cover smooth), temperature is 150 DEG C ± 3 DEG C, yard/minute of speed 65;
G. second glue spreading:Coating is that raw material preparation viscosity is 10000 with glue with PUR and methyl esters;If it is desired to gold size, silver
, it is necessary to just carry out the coating of gold size or elargol after bottoming one time again when glue or other coloring agents;
H. finished product sizing:Door width is allocated on request, and temperature is 120~130 DEG C, and speed is 45 yards/minute, and sky determines place can not be sprinkled
Water;Packaging is finished product on request after finished product sizing.
From the above-mentioned description of this invention, compared to the prior art, the invention has the advantages that:By the present invention
Color-changing printing technique prepare umbrella cloth can't see flower pattern under dry state, show flower pattern under hygrometric state, show unique characteristics so that
Product possesses the good market competitiveness;In addition, special printing technology of the invention is standardized production, technological process temperature,
So that the uniformity of product is very strong, obtained excellent product quality, stable performance, with more than 3 years service life.
Specific embodiment
Implementation method one
The plain color color-changing printing umbrella cloth of present embodiment is produced by following techniques, and the technique is following by what is carried out successively
Step is constituted:
A. dye:Plain color A grades of fabric is dyed into required base color;Fabric is confirmed by customer order, and carries out more than 10%
Sampling observation, prevents fabric cloth cover from having the defective products such as billet, crosspiece and knot;The coloured light requirement of dyeing is accurate, and fastness meets the requirements, and prevents
The only bad order such as cloth cover color dot, pollution, color-changing printing can not be using the fabric that changes colour;
B. preparation sizing:Door width applies setting agent to carry out preparing sizing at the place of specifying on request, and sky determines place and is unable to water-sprinkling, and sky is fixed
It refer to the position for not applying setting agent;Check on fabric appearance quality, there is that color dot, dyeing defect etc. are bad must not to enter subsequent processing;
C. a gluing:By PUR(It is commonly called as virgin rubber, film), methyl esters is with 21:4 ratio is mixed to prepare with glue, virgin rubber glue
Unify viscosity, the addition precision prescribed of methyl esters is accurate;Primer first is coated with the fabric of preparation sizing, is coated with glue;Bottom
It is 17000~18000 PUR that glue uses viscosity, uses coloring agent as primer during dark color painting elargol, and speed is 60 yards/point
Clock, needs drying;It is required that glue can not front, glue surface uniformity thoroughly, prevent adhesive tape etc.;Need to check that cloth cover is in 200 yards of start
No seep through;
D. stamp:Former paste is made using sodium alginate, the water repellent that 7% is added by weight proportion is tuned into the printing paste that viscosity is 5000;
The non-coated face of plain color of coating is first imprinted on by the examination of ready-made printing paste, with 130~140 DEG C, is then totally dried with reduction cleaning
It is dry, see fabric quality, first, printing opacity cannot see that flower pattern, second, printed side not descend water to cannot see that flower pattern, and the 3rd, lower water is vertical
Flowering type;Sample printing paste up to standard is carried out by stamp by printing machine again, printing machine speed is 38 yards/minute, and stamp passes through
Temperature is that 130~140 DEG C of drying room is dried;Stamp cropping to check in time cloth cover whether uniformity, lower machine product palpus
In time to washing machine washing sample, printing effect is determined;Leftover of bolt of cloth positive and negative will identify clear, and stamp cannot pass through into and out of cloth and not turn
Dynamic fabric guide roll, screw thread spread roller can not open friction glue surface, and stamp arc will swathe one layer of woven dacron to reduce friction hair
Heat, needs appropriate shutdown cooling when starting shooting for a long time, in order to avoid because heating produces micelle;
E. wash:Machine is washed in 2~3 hours by rinsing machine under stamp, can otherwise be produced and be creased;Health must before washing
Must cleaning in place, prevent booty to be bonded at cloth cover, during washing glue surface upward, prevent run side, flanging, crease, under confidential inspection be
It is no to produce micelle and other fabric quality problems;Washing process is that the grooves of a. first put flowing cool water;B. second and third, four, five grooves
Plus sodium hydrosulfite 2g/L, caustic soda 1g/L, temperature is 80~85 DEG C, and each groove of this step is necessary during 4000 yards or so of cloth cover of washing
Change water once, speed is 43 yards/minute;C. the 6th groove heating degree is 55~60 DEG C of warm water, and the 7th groove adds flowing cool water;D. dry
When dry, cloth cover keeps 70~80% aridity, prevents from excessively drying the micelle caused by friction;
F. sizing in the middle of:Door width is allocated on request, and temperature is 150 DEG C ± 3 DEG C, yard/minute of speed 65, fabric quality of checking on, such as
Having the quality problems such as pierced carving, micelle, pollution must not enter subsequent processing;
G. second glue spreading:Coating is that raw material preparation viscosity is 10000 with glue with PUR and methyl esters, it is impossible to penetrate into front;
Must check whether whether viscose glue, hydraulic pressure are up to standard and whether positive and negative applies mistake etc. when producing 200 yards;If it is desired to gold size, elargol or
, it is necessary to just carry out the coating of gold size or elargol after bottoming one time again during other coloring agents of person, golden, saturating silver-colored phenomenon is prevented;
H. finished product sizing:Gold size, elargol coating do not protect width(It is to keep width stabilization to protect width);Door width is allocated on request, temperature
It it is 120~130 DEG C, speed is 45 yards/minute, sky determines place and is unable to water-sprinkling;Packaging is finished product on request after finished product sizing.
Implementation method two
The plain color color-changing printing umbrella cloth of present embodiment is produced by following techniques, and the technique is following by what is carried out successively
Step is constituted:
A. dye:Plain color A grades of fabric is dyed into required base color;Fabric is confirmed by customer order, and carries out more than 10%
Sampling observation, prevents fabric cloth cover from having the defective products such as billet, crosspiece and knot;The coloured light requirement of dyeing is accurate, and fastness meets the requirements, and prevents
The only bad order such as cloth cover color dot, pollution, color-changing printing can not be using the fabric that changes colour;
B. preparation sizing:Door width applies setting agent to carry out preparing sizing at the place of specifying on request, and sky determines place and is unable to water-sprinkling, and sky is fixed
It refer to the position for not applying setting agent;Check on fabric appearance quality, there is that color dot, dyeing defect etc. are bad must not to enter subsequent processing;
C. a gluing:By PUR(It is commonly called as virgin rubber, film), methyl esters is with 20:4 ratio is mixed to prepare with glue, virgin rubber glue
Unify viscosity, the addition precision prescribed of methyl esters is accurate;Primer first is coated with the fabric of preparation sizing, is coated with glue;Bottom
It is 17000~18000 PUR that glue uses viscosity, uses coloring agent as primer during dark color painting elargol, and speed is 62 yards/point
Clock, needs drying;It is required that glue can not front, glue surface uniformity thoroughly, prevent adhesive tape etc.;Need to check that cloth cover is in 200 yards of start
No seep through;
D. stamp:Former paste is made using sodium alginate, the water repellent that 6% is added by weight proportion is tuned into the printing paste that viscosity is 4500;
The non-coated face of plain color of coating is first imprinted on by the examination of ready-made printing paste, with 130~140 DEG C, is then totally dried with reduction cleaning
It is dry, see fabric quality, first, printing opacity cannot see that flower pattern, second, printed side not descend water to cannot see that flower pattern, and the 3rd, lower water is vertical
Flowering type;Sample printing paste up to standard is carried out by stamp by printing machine again, printing machine speed is 35 yards/minute, and stamp passes through
Temperature is that 130~140 DEG C of drying room is dried;Stamp cropping to check in time cloth cover whether uniformity, lower machine product palpus
In time to washing machine washing sample, printing effect is determined;Leftover of bolt of cloth positive and negative will identify clear, and stamp cannot pass through into and out of cloth and not turn
Dynamic fabric guide roll, screw thread spread roller can not open friction glue surface, and stamp arc will swathe one layer of woven dacron to reduce friction hair
Heat, needs appropriate shutdown cooling when starting shooting for a long time, in order to avoid because heating produces micelle;
E. wash:Machine is washed in 2~3 hours by rinsing machine under stamp, can otherwise be produced and be creased;Health must before washing
Must cleaning in place, prevent booty to be bonded at cloth cover, during washing glue surface upward, prevent run side, flanging, crease, under confidential inspection be
It is no to produce micelle and other fabric quality problems;Washing process is that the grooves of a. first put flowing cool water;B. second and third, four grooves difference
Addition sodium hydrosulfite 2.3g/L, caustic soda 0.8g/L, temperature are 80~85 DEG C, each groove of this step during 4000 yards or so of washing cloth cover
Water must be changed once, speed is 45 yards/minute;C. the 5th groove heating degree is 55~60 DEG C of warm water, and the 6th groove adds flowing cold
Water;When d. drying, cloth cover keeps 70~80% aridity, prevents from excessively drying the micelle caused by friction;
F. sizing in the middle of:Door width is allocated on request, and temperature is 150 DEG C ± 3 DEG C, yard/minute of speed 63, fabric quality of checking on, such as
Having the quality problems such as pierced carving, micelle, pollution must not enter subsequent processing;
G. second glue spreading:Coating is that raw material preparation viscosity is 9200 with glue with PUR and methyl esters, it is impossible to penetrate into front;It is raw
Must check whether whether viscose glue, hydraulic pressure are up to standard and whether positive and negative applies mistake etc. when producing 200 yards;If it is desired to gold size, elargol or
, it is necessary to just carry out the coating of gold size or elargol after bottoming one time again during other coloring agents, golden, saturating silver-colored phenomenon is prevented;
H. finished product sizing:Door width is allocated on request, and temperature is 120~130 DEG C, and speed is 45 yards/minute, and sky determines place can not be sprinkled
Water;Packaging is finished product on request after finished product sizing.
Implementation method three
The plain color color-changing printing umbrella cloth of present embodiment is produced by following techniques, and the technique is following by what is carried out successively
Step is constituted:
A. dye:Plain color A grades of fabric is dyed into required base color;Fabric is confirmed by customer order, and carries out more than 10%
Sampling observation, prevents fabric cloth cover from having the defective products such as billet, crosspiece and knot;The coloured light requirement of dyeing is accurate, and fastness meets the requirements, and prevents
The only bad order such as cloth cover color dot, pollution, color-changing printing can not be using the fabric that changes colour;
B. preparation sizing:Door width applies setting agent to carry out preparing sizing at the place of specifying on request, and sky determines place and is unable to water-sprinkling, and sky is fixed
It refer to the position for not applying setting agent;Check on fabric appearance quality, there is that color dot, dyeing defect etc. are bad must not to enter subsequent processing;
C. a gluing:By PUR(It is commonly called as virgin rubber, film), methyl esters is with 23:4 ratio is mixed to prepare with glue, virgin rubber glue
Unify viscosity, the addition precision prescribed of methyl esters is accurate;Primer first is coated with the fabric of preparation sizing, is coated with glue;Bottom
It is 17000~18000 PUR that glue uses viscosity, uses coloring agent as primer during dark color painting elargol, and speed is 55 yards/point
Clock, needs drying;It is required that glue can not front, glue surface uniformity thoroughly, prevent adhesive tape etc.;Need to check that cloth cover is in 200 yards of start
No seep through;
D. stamp:Former paste is made using sodium alginate, the water repellent that 8% is added by weight proportion is tuned into the printing paste that viscosity is 5000;
The non-coated face of plain color of coating is first imprinted on by the examination of ready-made printing paste, with 130~140 DEG C, is then totally dried with reduction cleaning
It is dry, see fabric quality, first, printing opacity cannot see that flower pattern, second, printed side not descend water to cannot see that flower pattern, and the 3rd, lower water is vertical
Flowering type;Sample printing paste up to standard is carried out by stamp by printing machine again, printing machine speed is 40 yards/minute, and stamp passes through
Temperature is that 130~140 DEG C of drying room is dried;Stamp cropping to check in time cloth cover whether uniformity, lower machine product palpus
In time to washing machine washing sample, printing effect is determined;Leftover of bolt of cloth positive and negative will identify clear, and stamp cannot pass through into and out of cloth and not turn
Dynamic fabric guide roll, screw thread spread roller can not open friction glue surface, and stamp arc will swathe one layer of woven dacron to reduce friction hair
Heat, needs appropriate shutdown cooling when starting shooting for a long time, in order to avoid because heating produces micelle;
E. wash:Machine is washed in 2~3 hours by rinsing machine under stamp, can otherwise be produced and be creased;Health must before washing
Must cleaning in place, prevent booty to be bonded at cloth cover, during washing glue surface upward, prevent run side, flanging, crease, under confidential inspection be
It is no to produce micelle and other fabric quality problems;Washing process is that the grooves of a. first put flowing cool water;B. second and third, four, five, six
Groove adds sodium hydrosulfite 1.7g/L, caustic soda 1.2g/L, and temperature is 80~85 DEG C, each groove of this step during 4000 yards or so of washing cloth cover
Water must be changed once, speed is 40 yards/minute;C. the 7th groove heating degree is 55~60 DEG C of warm water, and the 8th groove adds flowing cold
Water;When d. drying, cloth cover keeps 70~80% aridity, prevents from excessively drying the micelle caused by friction;
F. sizing in the middle of:Door width is allocated on request, and temperature is 150 DEG C ± 3 DEG C, yard/minute of speed 70, fabric quality of checking on, such as
Having the quality problems such as pierced carving, micelle, pollution must not enter subsequent processing;
G. second glue spreading:Coating is that raw material preparation viscosity is 11000 with glue with PUR and methyl esters, it is impossible to penetrate into front;
Must check whether whether viscose glue, hydraulic pressure are up to standard and whether positive and negative applies mistake etc. when producing 200 yards;If it is desired to gold size, elargol or
, it is necessary to just carry out the coating of gold size or elargol after bottoming one time again during other coloring agents of person, golden, saturating silver-colored phenomenon is prevented;
H. finished product sizing:Door width is allocated on request, and temperature is 120~130 DEG C, and speed is 45 yards/minute, and sky determines place can not be sprinkled
Water;Packaging is finished product on request after finished product sizing.
Implementation method four
The plain color color-changing printing umbrella cloth of present embodiment is produced by following techniques, and the technique is following by what is carried out successively
Step is constituted:
A. dye:Plain color A grades of fabric is dyed into required base color;Fabric is confirmed by customer order, and carries out more than 10%
Sampling observation, prevents fabric cloth cover from having the defective products such as billet, crosspiece and knot;The coloured light requirement of dyeing is accurate, and fastness meets the requirements, and prevents
The only bad order such as cloth cover color dot, pollution, color-changing printing can not be using the fabric that changes colour;
B. preparation sizing:Door width applies setting agent to carry out preparing sizing at the place of specifying on request, and sky determines place and is unable to water-sprinkling, and sky is fixed
It refer to the position for not applying setting agent;Check on fabric appearance quality, there is that color dot, dyeing defect etc. are bad must not to enter subsequent processing;
C. a gluing:By PUR(It is commonly called as virgin rubber, film), methyl esters is with 22:4 ratio is mixed to prepare with glue, virgin rubber glue
Unify viscosity, the addition precision prescribed of methyl esters is accurate;Primer first is coated with the fabric of preparation sizing, is coated with glue;Bottom
It is 17000~18000 PUR that glue uses viscosity, uses coloring agent as primer during dark color painting elargol, and speed is 58 yards/point
Clock, needs drying;It is required that glue can not front, glue surface uniformity thoroughly, prevent adhesive tape etc.;Need to check that cloth cover is in 200 yards of start
No seep through;
D. stamp:Former paste is made using sodium alginate, the water repellent that 7% is added by weight proportion is tuned into the printing paste that viscosity is 5300;
The non-coated face of plain color of coating is first imprinted on by the examination of ready-made printing paste, with 130~140 DEG C, is then totally dried with reduction cleaning
It is dry, see fabric quality, first, printing opacity cannot see that flower pattern, second, printed side not descend water to cannot see that flower pattern, and the 3rd, lower water is vertical
Flowering type;Sample printing paste up to standard is carried out by stamp by printing machine again, printing machine speed is 36 yards/minute, and stamp passes through
Temperature is that 130~140 DEG C of drying room is dried;Stamp cropping to check in time cloth cover whether uniformity, lower machine product palpus
In time to washing machine washing sample, printing effect is determined;Leftover of bolt of cloth positive and negative will identify clear, and stamp cannot pass through into and out of cloth and not turn
Dynamic fabric guide roll, screw thread spread roller can not open friction glue surface, and stamp arc will swathe one layer of woven dacron to reduce friction hair
Heat, needs appropriate shutdown cooling when starting shooting for a long time, in order to avoid because heating produces micelle;
E. wash:Machine is washed in 2~3 hours by rinsing machine under stamp, can otherwise be produced and be creased;Health must before washing
Must cleaning in place, prevent booty to be bonded at cloth cover, during washing glue surface upward, prevent run side, flanging, crease, under confidential inspection be
It is no to produce micelle and other fabric quality problems;Washing process is that the grooves of a. first put flowing cool water;B. second and third groove adds insurance
Powder 1.8g/L, caustic soda 0.9g/L, temperature are 80~85 DEG C, and each groove of this step must be changed during 4000 yards or so of cloth cover of washing
Once, speed is 44 yards/minute to water;C. the 4th groove heating degree is 55~60 DEG C of warm water, and the 5th groove adds flowing cool water;D. dry
When, cloth cover keeps 70~80% aridity, prevents from excessively drying the micelle caused by friction;
F. sizing in the middle of:Door width is allocated on request, and temperature is 150 DEG C ± 3 DEG C, yard/minute of speed 68, fabric quality of checking on, such as
Having the quality problems such as pierced carving, micelle, pollution must not enter subsequent processing;
G. second glue spreading:Coating is that raw material preparation viscosity is 10500 with glue with PUR and methyl esters, it is impossible to penetrate into front;
Must check whether whether viscose glue, hydraulic pressure are up to standard and whether positive and negative applies mistake etc. when producing 200 yards;If it is desired to gold size, elargol or
, it is necessary to just carry out the coating of gold size or elargol after bottoming one time again during other coloring agents of person, golden, saturating silver-colored phenomenon is prevented;
H. finished product sizing:Door width is allocated on request, and temperature is 120~130 DEG C, and speed is 46 yards/minute, and sky determines place can not be sprinkled
Water;Packaging is finished product on request after finished product sizing.
Specific embodiment of the invention is above are only, but design concept of the invention is not limited thereto, it is all to utilize this
Design carries out the change of unsubstantiality to the present invention, all should belong to the behavior for invading the scope of the present invention.
Claims (6)
1. plain color umbrella cloth color-changing printing technique, it is characterised in that including the following step for carrying out successively:
A. dye:Plain color A grades of fabric is dyed into required base color;
B. preparation sizing:Door width carries out preparing sizing on request, and sky determines place and is unable to water-sprinkling;
C. a gluing:By PUR, methyl esters with 20~23:4 ratio is mixed to prepare with glue;First on the fabric of preparation sizing
Coating primer, is coated with glue;Primer use viscosity for 17000~18000 PUR, speed be 55~62 yards/minute, dry
It is dry;
D. stamp:Former paste is made using sodium alginate, it is 4500~5500 that the water repellent of addition 6~8% by weight proportion is tuned into viscosity
Printing paste;Stamp is carried out using the printing paste by printing machine, printing machine speed is 35~40 yards/minute, and stamp is by temperature
The drying room spent for 130~140 DEG C is dried;
E. wash:Washed by rinsing machine in machine 2~3 hours under stamp, glue surface is upward during washing;Washing process is,
A. the first groove puts flowing cool water;B. second adds 1.7~2.3g/L of sodium hydrosulfite, 0.8~1.2g/L of caustic soda to N grooves, and temperature is 80
~85 DEG C, each groove of this step must change water once during 4000 yards or so of cloth cover of washing, and speed is 40~45 yards/minute;
C. N+1 grooves heating degree is 55~60 DEG C of warm water, and N+2 grooves add flowing cool water;When d. drying, cloth cover keeps 70~80%
Aridity;
F. sizing in the middle of:Door width is allocated on request, and temperature is 150 DEG C ± 3 DEG C, yard/minute of speed 63~70;
G. second glue spreading:Coating is that raw material preparation viscosity is 9200~11000 with glue with PUR and methyl esters;
H. finished product sizing:Door width is allocated on request, and temperature is 120~130 DEG C, and speed is 40~48 yards/minute, and sky determines place can not
Water-sprinkling;It is finished product after finished product sizing.
2. plain color umbrella cloth color-changing printing technique as claimed in claim 1, it is characterised in that including the following steps for carrying out successively
Suddenly:
A. dye:Plain color A grades of fabric is dyed into required base color;
B. preparation sizing:Door width carries out preparing sizing on request, and sky determines place and is unable to water-sprinkling;
C. a gluing:By PUR, methyl esters with 21:4 ratio is mixed to prepare with glue;First it is coated with the fabric of preparation sizing
Primer, is coated with glue;Primer use viscosity for 17000~18000 PUR, speed be 60 yards/minute, drying;
D. stamp:Former paste is made using sodium alginate, the water repellent that 7% is added by weight proportion is tuned into the printing paste that viscosity is 5000;
Stamp is carried out using the printing paste by printing machine, printing machine speed is 35~40 yards/minute, stamp by temperature be 130~
140 DEG C of drying room is dried;
E. wash:Washed by rinsing machine in machine 2~3 hours under stamp, glue surface is upward during washing;Washing process is,
A. the first groove puts flowing cool water;B. second and third, four, five grooves add sodium hydrosulfite 2g/L, caustic soda 1g/L, temperature is 80~85 DEG C, washing
Each groove of this step must change water once during 4000 yards or so of cloth cover, and speed is 40~45 yards/minute;C. the 6th groove heating
The warm water for 55~60 DEG C is spent, the 7th groove adds flowing cool water;When d. drying, cloth cover keeps 70~80% aridity;
F. sizing in the middle of:Door width is allocated on request, and temperature is 150 DEG C ± 3 DEG C, yard/minute of speed 65;
G. second glue spreading:Coating is that raw material preparation viscosity is 10000 with glue with PUR and methyl esters;
H. finished product sizing:Door width is allocated on request, and temperature is 120~130 DEG C, and speed is 45 yards/minute, and sky determines place can not be sprinkled
Water;It is finished product after finished product sizing.
3. plain color umbrella cloth color-changing printing technique as claimed in claim 1, it is characterised in that:In coating process of step C,
Dark color uses coloring agent as primer when applying elargol.
4. plain color umbrella cloth color-changing printing technique as claimed in claim 1, it is characterised in that:In coating process of step C,
It is required that glue can not front thoroughly, glue surface is uniform;Start 200 yards in need check cloth cover whether seep through.
5. plain color umbrella cloth color-changing printing technique as claimed in claim 1, it is characterised in that:In step D revenue stamp processes, the leftover of bolt of cloth
Positive and negative will identify clear, and stamp cannot pass through the fabric guide roll not rotated into and out of cloth, and screw thread spread roller can not open friction glue
Face, stamp arc will swathe one layer of woven dacron to reduce frictional heating, and appropriate shutdown cooling is needed when starting shooting for a long time.
6. plain color umbrella cloth color-changing printing technique as claimed in claim 1, it is characterised in that:In step G second glue spreading operations,
If it is desired to, it is necessary to just carry out the coating of gold size or elargol after bottoming one time again when gold size, elargol or other coloring agents.