CN107059300A - A non-contact processing device and method for silk patterns - Google Patents

A non-contact processing device and method for silk patterns Download PDF

Info

Publication number
CN107059300A
CN107059300A CN201710377381.9A CN201710377381A CN107059300A CN 107059300 A CN107059300 A CN 107059300A CN 201710377381 A CN201710377381 A CN 201710377381A CN 107059300 A CN107059300 A CN 107059300A
Authority
CN
China
Prior art keywords
silk
silk pattern
treatment
pattern
fibroin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201710377381.9A
Other languages
Chinese (zh)
Other versions
CN107059300B (en
Inventor
李世超
黄阳阳
张振威
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Suzhou Vocational University
Original Assignee
Suzhou Vocational University
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Suzhou Vocational University filed Critical Suzhou Vocational University
Priority to CN201710377381.9A priority Critical patent/CN107059300B/en
Publication of CN107059300A publication Critical patent/CN107059300A/en
Application granted granted Critical
Publication of CN107059300B publication Critical patent/CN107059300B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种丝绸纹样的非接触式处理装置及方法,处理装置,包括处理箱和防雾罩;处理箱内部的底面设置有红外加热器;处理箱的下部设置有吸风口;处理箱内部的上部设置有支撑架;支撑架上设置有网状处理架;网状处理架上设置有压框;处理箱的上端设置有防雾罩;防雾罩内部的上端设置有喷雾装置;喷雾装置的一端连接输液杆;输液杆上设置有液用量控制器;液用量控制器外连微型加压泵;喷雾装上设置有喷雾头。处理方法包括以下步骤:1)制备处理液;2)使用丝绸纹样的非接触式处理装置处理无需支架加固的丝绸纹样或需先支架加固的丝绸纹样。本发明可以有效避免接触丝绸纹样带来的损坏,操作简便,保护丝绸纹样本身的样貌,实用性强。

The invention discloses a non-contact processing device and method for silk patterns. The processing device includes a processing box and an anti-fog cover; an infrared heater is arranged on the bottom surface inside the processing box; The upper part of the interior is provided with a support frame; the support frame is provided with a mesh processing frame; the mesh processing frame is provided with a pressure frame; the upper end of the processing box is provided with an anti-fog cover; One end of the device is connected with an infusion rod; the infusion rod is provided with a liquid dosage controller; the liquid dosage controller is externally connected with a micro pressurized pump; the spray device is provided with a spray head. The treatment method includes the following steps: 1) preparing a treatment liquid; 2) using a non-contact silk pattern treatment device to process the silk pattern that does not need to be reinforced by a support or the silk pattern that needs to be reinforced by a support first. The invention can effectively avoid the damage caused by touching the silk pattern, is easy to operate, protects the appearance of the silk pattern itself, and has strong practicability.

Description

一种丝绸纹样的非接触式处理装置及方法A non-contact processing device and method for silk patterns

技术领域technical field

本发明涉及一种丝绸纹样的处理装置及方法,尤其是一种丝绸纹样的非接触式的处理装置及方法。The invention relates to a processing device and method for silk patterns, in particular to a non-contact processing device and method for silk patterns.

背景技术Background technique

丝绸纹样是丝绸档案中珍贵的历史资料,它记录着产品的风貌,加工的工艺和时代的特征,不可再生,需长期保存。但丝绸属蛋白质有机材料,日常受微生物和光照作用,其质地极容易老化。因此,在保存中要进行相应的防霉和抗光处理。丝绸纹样一般都有一定的年代,有的历史甚至十分悠久,质地强度较弱,采用常规的接触式浸轧处理方式往往会对纹样造成二次损害。本技术提供了一种非接触式的丝绸纹样处理方法和处理装置,从而避免丝绸纹样在处理时的自身伤害。Silk patterns are precious historical materials in silk archives. They record the appearance of products, processing techniques and characteristics of the times. They are non-renewable and need to be preserved for a long time. However, silk is a protein organic material, and its texture is very easy to age due to the daily action of microorganisms and light. Therefore, corresponding anti-mildew and anti-light treatments should be carried out during storage. Silk patterns generally have a certain age, and some have a very long history, and the texture strength is weak. The conventional contact padding treatment will often cause secondary damage to the pattern. The technology provides a non-contact silk pattern processing method and processing device, thereby avoiding self-injury of the silk pattern during processing.

发明内容Contents of the invention

针对上述存在的技术问题,本发明的目的是:提出了一种有效保护丝绸纹样本身,避免损坏的非接触式的处理装置及方法。In view of the above-mentioned technical problems, the object of the present invention is to propose a non-contact processing device and method that can effectively protect the silk pattern itself and avoid damage.

本发明的技术解决方案是这样实现的:一种丝绸纹样的非接触式处理装置,包括处理箱和防雾罩;所述处理箱内部的底面设置有红外加热器;所述处理箱的下部设置有吸风口;所述吸风口连接吸风器;所述处理箱内部的上部设置有支撑架;所述支撑架上设置有网状处理架;所述网状处理架上设置有压框;所述处理箱的上端设置有防雾罩;所述防雾罩内部的上端设置有喷雾装置;所述喷雾装置的一端连接输液杆;所述输液杆上设置有液用量控制器;所述液用量控制器外连微型加压泵;所述喷雾装上设置有喷雾头;所述喷雾装置绕着输液杆旋转。The technical solution of the present invention is achieved as follows: a non-contact processing device for silk patterns, including a processing box and an anti-fog cover; the bottom surface inside the processing box is provided with an infrared heater; There is an air suction port; the air suction port is connected to the air aspirator; the upper part of the processing box is provided with a support frame; the support frame is provided with a mesh processing frame; the mesh processing frame is provided with a pressure frame; The upper end of the treatment box is provided with an anti-fog cover; the upper end inside the anti-fog cover is provided with a spray device; one end of the spray device is connected to an infusion rod; the infusion rod is provided with a liquid dosage controller; The controller is externally connected with a miniature booster pump; the spray device is provided with a spray head; the spray device rotates around the infusion rod.

优选的,所述吸风口分布在处理箱前后左右四个侧面上;吸风口至少有六个。Preferably, the air suction ports are distributed on the front, rear, left, and right sides of the treatment box; there are at least six air suction ports.

优选的,所述喷雾装置包括四根与输液杆平行的喷雾管;四根喷雾管分布于输液杆的上、下、左、右的方位上;所述喷雾头均匀分布于喷雾管上;每根喷雾管上至少有六个喷雾头。Preferably, the spray device includes four spray pipes parallel to the infusion rod; the four spray pipes are distributed on the upper, lower, left and right directions of the infusion rod; the spray heads are evenly distributed on the spray pipes; There are at least six spray heads on the root spray pipe.

优选的,所述网状处理架的丝网用加捻尼龙丝线穿成。Preferably, the wire mesh of the mesh processing frame is threaded with twisted nylon threads.

优选的,所述压框的内外部尺寸与丝网处理架的内外尺寸相同。Preferably, the internal and external dimensions of the press frame are the same as those of the screen processing frame.

一种丝绸纹样的非接触式处理方法,包括以下步骤:A non-contact method for processing silk patterns, comprising the following steps:

1)制备处理液:用去离子水按以下成份、配比配制防霉或抗光处理液;1) Preparation of treatment solution: use deionized water to prepare anti-mildew or anti-light treatment solution according to the following ingredients and proportions;

防霉处理液:防霉剂:1-5 wt%;丝素粉:1-8 wt%;溶剂: 去离子水;Anti-mold treatment liquid: anti-mold agent: 1-5 wt%; silk fibroin powder: 1-8 wt%; solvent: deionized water;

抗光处理液:抗光剂:5-15 wt%;丝素粉:1-8 wt%;溶剂: 去离子水;Anti-light treatment liquid: anti-light agent: 5-15 wt%; silk fibroin powder: 1-8 wt%; solvent: deionized water;

2)使用丝绸纹样的非接触式处理装置处理无需支架加固的丝绸纹样或需先支架加固的丝绸纹样;2) Use a non-contact processing device for silk patterns to process silk patterns that do not need support reinforcement or silk patterns that need support reinforcement first;

所述使用丝绸纹样的非接触式处理装置处理无需支架加固的丝绸纹样的具体步骤如下:The specific steps of using the non-contact processing device for silk patterns to process silk patterns that do not require support reinforcement are as follows:

A、放置丝绸纹样:将丝绸纹样平放在处理箱中的网状处理架上,反面朝上;A. Place the silk pattern: place the silk pattern flat on the mesh processing rack in the processing box, with the reverse side facing up;

B、喷雾处理:用配置好的处理液在丝绸纹样的反面进行喷雾处理;喷雾时喷雾装置的转速为20—40转/分,由处理液用量控制器进行控制,一般液用量控制在150—350ml/m2内;B. Spray treatment: use the configured treatment liquid to spray on the reverse side of the silk pattern; when spraying, the speed of the spray device is 20-40 rpm, controlled by the treatment liquid dosage controller, and the general liquid dosage is controlled at 150- Within 350ml/ m2 ;

C、吸风处理:喷雾完成后,压框压在网状处理架上,吸风以微风方式进行,吸风量一般控制在0.5—1.5m3/h之间,吸风时间控制在60—120分钟;C. Suction treatment: After the spraying is completed, the pressure frame is pressed on the mesh treatment frame, and the suction is carried out in a breeze. The suction volume is generally controlled between 0.5-1.5m 3 /h, and the suction time is controlled at 60-120 minute;

D、干燥处理:吸风完成后,开启红外干燥器进行干燥,干燥温度一般在35—60℃之间,时间为20—40分钟;D. Drying treatment: After the air suction is completed, turn on the infrared dryer to dry. The drying temperature is generally between 35-60°C and the time is 20-40 minutes;

E、将丝绸纹样正面朝上放置,并依次进行喷雾处理、吸风处理、干燥处理;E. Place the silk pattern face up, and carry out spray treatment, suction treatment and drying treatment in sequence;

F、将丝绸纹样的正、反面都进行了喷雾处理、吸风处理、干燥处理之后,进行自然平衡24h;F. After the front and back of the silk pattern are sprayed, sucked and dried, they are naturally balanced for 24 hours;

所述使用丝绸纹样的非接触式处理装置处理需先支架加固的丝绸纹样的具体步骤如下:The specific steps of using the non-contact processing device for silk patterns to process the silk patterns that need to be reinforced first are as follows:

A、加固材料处理:将丝绸纹样浸入防霉或抗光处理液内,待充分湿润后取出,放在平板上用橡胶滚筒进行正反面的滚轧操作;经处理液“二浸二轧”后,进行自然干燥备用;A. Reinforcing material treatment: immerse the silk pattern in anti-mildew or anti-light treatment liquid, take it out after it is fully wet, put it on a flat plate and use a rubber roller to roll the front and back sides; , carry out natural drying for standby;

B、配制丝素胶乳液:按以下成份、配比配制丝素胶乳液:B. Prepare silk fibroin latex: prepare silk fibroin latex according to the following ingredients and proportions:

丙烯酸聚合物乳液:30-45 wt%;丝素粉:1-4 wt%溶剂:去离子水;Acrylic polymer emulsion: 30-45 wt%; silk fibroin powder: 1-4 wt% solvent: deionized water;

所述丙烯酸聚合物乳液中各单体的重量比为:甲基丙烯酸甲酯:10-15 %,丙烯酸丁酯:75-85 %;丙烯酸:3-7 %;丙烯酸-2-羟乙酯:2-5 %;The weight ratio of each monomer in the acrylic acid polymer emulsion is: methyl methacrylate: 10-15%, butyl acrylate: 75-85%; acrylic acid: 3-7%; 2-hydroxyethyl acrylate: 2-5%;

C、支架加固处理:在PET低粘性薄膜材料表面设置支架制作工作区域,在工作区域内均匀涂覆已制备的丝素胶乳液,丝素胶乳液的用量在8-10ml;用一次性注射器吸取8-10mL丝素胶乳液,均匀滴到低粘性薄膜材料工作区域内;用羊毫毛刷,在工作区域内对乳液进行横向和纵向的反复涂刷,使丝素胶乳液在区域内分布均匀,涂刷时的环境温度为27-29℃;在涂刷过程中,丝素胶乳液中的乳白色消失时,在PET低粘性薄膜材料上的丝素胶膜初步达到成型;将经过浸轧处理的丝绸支架材料粘贴到工作区域内的丝素胶膜表面,用橡胶滚筒在丝绸支架材料上进行滚压,橡胶滚筒表面的硬度为70-75,滚压压力为15-20kg;将丝绸支架材料从PET低粘性薄膜材料上剥离后,丝素胶膜被均匀且完整地粘着在丝绸支架材料表面形成加固支架;将需要加固丝绸纹样平放在光滑的平板表面,反面朝上,四周用压条固定;将加固支架带有丝素胶膜的一面压覆到丝绸纹样的反面,并用橡胶滚筒进行滚动加压,橡胶滚筒表面的硬度为70-75,加压压力为 15-20kg;压覆平整均匀后将加固后的丝绸纹样移置平整的工作台上进行24h的平衡,平衡温度为常温;C. Bracket reinforcement treatment: set up a working area for bracket production on the surface of PET low-viscosity film material, and evenly coat the prepared silk fibroin emulsion in the working area. The dosage of silk fibroin emulsion is 8-10ml; absorb it with a disposable syringe 8-10mL silk fibroin glue emulsion is evenly dropped into the working area of the low-viscosity film material; use a wool brush to repeatedly brush the emulsion horizontally and vertically in the working area, so that the silk fibroin glue emulsion is evenly distributed in the area, The ambient temperature during painting is 27-29°C; during the painting process, when the milky white color in the silk fibroin latex disappears, the silk fibroin film on the PET low-viscosity film material is initially formed; The silk support material is pasted on the surface of the silk fibroin film in the working area, and the rubber roller is used to roll on the silk support material. The hardness of the surface of the rubber roller is 70-75, and the rolling pressure is 15-20kg; After peeling off the PET low-adhesive film material, the silk fibroin film is evenly and completely adhered to the surface of the silk support material to form a reinforcement support; place the silk pattern that needs to be reinforced on a smooth flat surface, with the reverse side facing up, and fix it with pressure strips around it; Lay the side of the reinforcing bracket with the silk fibroin film on the reverse side of the silk pattern, and roll and press with a rubber roller. The surface hardness of the rubber roller is 70-75, and the pressing pressure is 15-20kg; Place the reinforced silk pattern on a flat workbench for 24 hours of balance, and the balance temperature is normal temperature;

D、放置丝绸纹样:将经过支架加固处理的丝绸纹样平放在处理箱中的网状处理架上,正面朝上;D. Place the silk pattern: put the silk pattern that has been reinforced by the bracket on the mesh processing rack in the processing box, with the front facing up;

E、喷雾处理:用配置好的处理液在丝绸纹样的反面进行喷雾处理;喷雾时喷雾装置的转速为20—40转/分,由处理液用量控制器进行控制,一般液用量控制在150—350ml/m2内;E. Spray treatment: use the configured treatment liquid to spray on the reverse side of the silk pattern; when spraying, the speed of the spray device is 20-40 rpm, controlled by the treatment liquid dosage controller, and the general liquid dosage is controlled at 150- Within 350ml/ m2 ;

F、吸风处理:喷雾完成后,压框压在网状处理架上,吸风以微风方式进行,吸风量一般控制在0.5—1.5m3/h之间,吸风时间控制在60—120分钟;F. Suction treatment: After the spraying is completed, the pressure frame is pressed on the mesh treatment frame, and the suction is carried out in a breeze. The suction volume is generally controlled between 0.5-1.5m 3 /h, and the suction time is controlled at 60-120 minute;

G、干燥处理:吸风完成后,开启红外干燥器进行干燥,干燥温度一般在35—60℃之间,时间为20—40分钟;G. Drying treatment: After the suction is completed, turn on the infrared dryer to dry. The drying temperature is generally between 35-60°C and the time is 20-40 minutes;

H、将经过干燥处理后的丝绸纹样,进行自然平衡24h。H. Naturally balance the dried silk patterns for 24 hours.

由于上述技术方案的运用,本发明与现有技术相比具有下列优点:Due to the application of the above-mentioned technical solution, the present invention has the following advantages compared with the prior art:

本发明的一种丝绸纹样的非接触式处理装置及方法,可以有效避免接触丝绸纹样带来的损坏,且设计合理,操作简便,非接触式的处理方式,保护丝绸纹样本身的样貌,实用性强。A non-contact processing device and method for silk patterns of the present invention can effectively avoid damage caused by contact with silk patterns, and is reasonable in design, easy to operate, non-contact processing method, protects the appearance of silk patterns itself, and is practical Strong.

附图说明Description of drawings

下面结合附图对本发明技术方案作进一步说明:Below in conjunction with accompanying drawing, technical solution of the present invention will be further described:

附图1为本发明的一种丝绸纹样的非接触式处理装置及方法的处理装置的主要结构示意图;Accompanying drawing 1 is the main structure schematic diagram of the processing device of a kind of non-contact processing device and method of silk pattern of the present invention;

附图2为附图1中A-A截面示意图;Accompanying drawing 2 is A-A sectional schematic diagram in accompanying drawing 1;

附图3为发明的一种丝绸纹样的非接触式处理装置及方法的处理装置的喷雾装置的结构示意图;Accompanying drawing 3 is the structure schematic diagram of the spraying device of the non-contact treatment device and method of the invention of a silk pattern;

附图4为本发明的一种丝绸纹样的非接触式处理装置及方法的处理装置的网状处理架的结构示意图。Accompanying drawing 4 is a schematic structural diagram of a mesh processing frame of a non-contact processing device and method for silk patterns according to the present invention.

具体实施方式detailed description

下面结合附图来说明本发明。The present invention is described below in conjunction with accompanying drawing.

如附图1-4所示为本发明所述的一种丝绸纹样的非接触式处理装置,包括处理箱1和防雾罩2;所述处理箱1内部的底面设置有红外加热器3;所述处理箱1的下部设置有吸风口4;所述吸风口4连接吸风器;所述处理箱1内部的上部设置有支撑架5;所述支撑架5上设置有网状处理架6;所述网状处理架6上设置有压框7;所述处理箱1的上端设置有防雾罩2;所述防雾罩2内部的上端设置有喷雾装置8;所述喷雾装置8的一端连接输液杆9;所述输液杆9上设置有液用量控制器10;所述液用量控制器10,外连微型加压泵;所述喷雾装置8上设置有喷雾头11;所述喷雾装置8绕着输液杆9旋转;所述吸风口4分布在处理箱1前后左右四个侧面上;吸风口4至少有六个;所述喷雾装置8包括四根与输液杆9平行的喷雾管12;四根喷雾管12分布于输液杆9的上、下、左、右的方位上;所述喷雾头11均匀分布于喷雾管12上;每根喷雾管12上至少有六个喷雾头11;所述网状处理架6的丝网用加捻尼龙丝线穿成,所述加捻尼龙丝线以20mm*20mm的网孔穿成,尼龙丝线粗细为300D,加捻捻度为4T/cm;液用量由液用量控制器10控制,加压采用微型加压泵进行加压;所述压框7的内外部尺寸与丝网处理架6的内外尺寸相同。As shown in accompanying drawing 1-4, it is a kind of non-contact treatment device of silk pattern according to the present invention, comprises treatment box 1 and anti-fog cover 2; The bottom surface inside described treatment box 1 is provided with infrared heater 3; The bottom of the processing box 1 is provided with a suction port 4; the suction port 4 is connected to a suction device; the upper part of the processing box 1 is provided with a support frame 5; the support frame 5 is provided with a mesh processing frame 6 ; The mesh processing frame 6 is provided with a pressure frame 7; the upper end of the treatment box 1 is provided with an anti-fog cover 2; the upper end of the anti-fog cover 2 inside is provided with a spray device 8; One end is connected with an infusion rod 9; the infusion rod 9 is provided with a liquid dosage controller 10; the liquid dosage controller 10 is externally connected with a micro pressure pump; the spray device 8 is provided with a spray head 11; The device 8 rotates around the infusion rod 9; the air suction port 4 is distributed on the front, rear, left, and right sides of the processing box 1; there are at least six air suction ports 4; the spray device 8 includes four spray pipes parallel to the infusion rod 9 12; four spray pipes 12 are distributed on the upper, lower, left and right directions of the infusion rod 9; the spray heads 11 are evenly distributed on the spray pipes 12; each spray pipe 12 has at least six spray heads 11 The screen of the mesh processing frame 6 is threaded with twisted nylon thread, and the twisted nylon thread is threaded with a mesh of 20mm*20mm, and the thickness of the nylon thread is 300D, and the twisting degree is 4T/cm; The consumption is controlled by the liquid consumption controller 10, and the pressurization adopts a micro-boosting pump to pressurize;

一种丝绸纹样的非接触式处理方法,包括以下步骤:A non-contact method for processing silk patterns, comprising the following steps:

1)制备处理液:用去离子水按以下成份、配比配制防霉或抗光处理液;1) Preparation of treatment solution: use deionized water to prepare anti-mildew or anti-light treatment solution according to the following ingredients and proportions;

防霉处理液:防霉剂:1-5 wt%;丝素粉:1-8 wt%;溶剂: 去离子水;Anti-mold treatment liquid: anti-mold agent: 1-5 wt%; silk fibroin powder: 1-8 wt%; solvent: deionized water;

抗光处理液:抗光剂:5-15 wt%;丝素粉:1-8 wt%;溶剂:去离子水;Anti-light treatment liquid: anti-light agent: 5-15 wt%; silk fibroin powder: 1-8 wt%; solvent: deionized water;

2)使用丝绸纹样的非接触式处理装置处理无需支架加固的丝绸纹样或需先支架加固的丝绸纹样;2) Use a non-contact processing device for silk patterns to process silk patterns that do not need support reinforcement or silk patterns that need support reinforcement first;

所述使用丝绸纹样的非接触式处理装置处理无需支架加固的丝绸纹样的具体步骤如下:对于一些具有一定自身强度的纹样,一般不作支架加固,这时纹样的处理可以采用正反面喷雾处理液的方法进行;The specific steps of using the non-contact processing device for silk patterns to process silk patterns that do not need support reinforcement are as follows: for some patterns with certain self-strength, generally no support is used for reinforcement. method to proceed;

A、放置丝绸纹样:首先打开防雾罩2,将丝绸纹样平放在处理箱1中的网状处理架6上,反面朝上,改好防雾罩2;A. Place the silk pattern: first open the anti-fog cover 2, put the silk pattern flat on the mesh processing frame 6 in the processing box 1, with the reverse side facing up, and change the anti-fog cover 2;

B、喷雾处理:根据防霉还是抗光不同的需求,用配置好的处理液在纹样的反面进行喷雾处理;喷雾时喷雾装置8的转速为20—40转/分,由处理液用量控制器10进行控制,一般液用量控制在150—350ml/m2内;B. Spray treatment: According to the different needs of anti-mildew or anti-light, use the configured treatment liquid to spray on the reverse side of the pattern; when spraying, the speed of the spray device 8 is 20-40 rpm, controlled by the treatment liquid dosage controller 10 for control, the general liquid dosage is controlled within 150-350ml/ m2 ;

C、吸风处理:丝绸纹样需对准网状处理架6上的丝网部分,压框7压在网状处理架6保证纹样的四周正好压住纹样,在吸风过程中防止纹样移动,吸风以微风方式进行,吸风量一般控制在0.5—1.5m3/h之间,吸风时间控制在60—120分钟;C. Suction treatment: the silk pattern needs to be aligned with the silk screen part on the mesh processing frame 6, and the pressure frame 7 is pressed on the mesh processing frame 6 to ensure that the pattern is just pressed around the pattern, and the pattern is prevented from moving during the suction process. The air suction is carried out in a breeze mode, the air suction volume is generally controlled between 0.5-1.5m 3 /h, and the suction time is controlled at 60-120 minutes;

D、干燥处理:吸风完成后,开启红外干燥器进行干燥,干燥温度一般在35—60℃之间,时间为20—40分钟;D. Drying treatment: After the air suction is completed, turn on the infrared dryer to dry. The drying temperature is generally between 35-60°C and the time is 20-40 minutes;

E、干燥处理完成后,将丝绸纹样正面朝上放置,并依次进行喷雾处理、吸风处理、干燥处理;E. After the drying treatment is completed, place the silk pattern face up, and then carry out spray treatment, suction treatment and drying treatment in sequence;

F、将丝绸纹样的正、反面都进行了喷雾处理、吸风处理、干燥处理之后,进行自然平衡24h,完成对丝绸纹样的非接触式处理;F. After the front and back of the silk pattern are sprayed, sucked and dried, they are naturally balanced for 24 hours to complete the non-contact treatment of the silk pattern;

所述使用丝绸纹样的非接触式处理装置处理需先支架加固的丝绸纹样的具体步骤如下:对于一些自身强度不够的纹样,不能直接进行非接触处理,首先需对纹样进行加固;The specific steps of using the non-contact processing device for silk patterns to process silk patterns that need to be reinforced by supports are as follows: for some patterns that are not strong enough, non-contact processing cannot be directly performed, and the patterns need to be reinforced first;

A、加固材料处理:将丝绸支架材料浸入防霉或抗光处理液内,待充分湿润后取出,放在平板上用橡胶滚筒进行正反面的滚轧操作;经处理液“二浸二轧”后,进行自然干燥备用;A. Reinforcement material treatment: Immerse the silk support material in the anti-mildew or anti-light treatment liquid, take it out after it is fully wet, put it on a flat plate and use a rubber roller to perform rolling operations on the front and back sides; after the treatment liquid, "two dipping and two rolling" After that, carry out natural drying for subsequent use;

B、配制丝素胶乳液:按以下成份、配比配制丝素胶乳液:B. Prepare silk fibroin latex: prepare silk fibroin latex according to the following ingredients and proportions:

丙烯酸聚合物乳液:30-45 wt%;丝素粉:1-4 wt%溶剂:去离子水;Acrylic polymer emulsion: 30-45 wt%; silk fibroin powder: 1-4 wt% solvent: deionized water;

所述丙烯酸聚合物乳液中各单体的重量比为:甲基丙烯酸甲酯:10-15 %,丙烯酸丁酯:75-85 %;丙烯酸:3-7 %;丙烯酸-2-羟乙酯:2-5 %;The weight ratio of each monomer in the acrylic acid polymer emulsion is: methyl methacrylate: 10-15%, butyl acrylate: 75-85%; acrylic acid: 3-7%; 2-hydroxyethyl acrylate: 2-5%;

C、支架加固处理:在PET低粘性薄膜材料表面设置25×34cm的支架制作工作区域,在该区域内均匀涂覆已制备的丝素胶乳液,根据支架的特点选择乳液的用量在8-10ml。具体操作步骤为:用一次性注射器吸取8-10mL丝素胶乳液,均匀滴到低粘性薄膜材料工作区域内;用毛长约10mm的羊毫毛刷,在工作区域内对乳液进行横向和纵向的反复涂刷,使丝素胶乳液在区域内分布均匀,涂刷时的环境温度为28℃左右;在涂刷过程中,丝素胶乳液中的水分逐步蒸发,乳液的乳白色逐步退去,待乳白色基本消失时,在PET低粘性薄膜材料上的丝素胶膜初步达到成型。紧接着将经处理的丝绸支架材料轻轻地粘贴到工作区域内的丝素胶膜表面,用橡胶滚筒在丝绸支架材料上均匀地进行滚压,橡胶滚筒表面的硬度为70-75之间,滚压的平均压力为15-20kg。反复滚压操作,直到平整均匀。由于丝素胶膜在丝绸支架材料与PET低粘性薄膜材料之间存在粘着应力的差异,丝绸支架材料从PET低粘性薄膜材料上剥离后,丝素胶膜被均匀且完整地粘着在丝绸支架材料表面形成加固支架。将需要加固的丝绸纹样平放在光滑的平板表面,反面朝上,四周用压条固定。将该加固支架带有丝素胶膜的一面轻轻地压覆到丝绸纹样的反面,并用橡胶滚筒进行滚动加压,橡胶滚筒表面的硬度为70-75之间,平均加压压力为 15-20kg。压覆平整均匀后将加固后的丝绸纹样移置平整的工作台上进行24h的平衡,平衡温度为常温;C. Stent reinforcement treatment: set a 25×34cm work area for stent production on the surface of the PET low-viscosity film material, and evenly coat the prepared silk fibroin emulsion in this area, and select the amount of emulsion to be 8-10ml according to the characteristics of the stent . The specific operation steps are: use a disposable syringe to absorb 8-10mL silk fibroin glue emulsion, and evenly drop it into the working area of the low-viscosity film material; Brush repeatedly to make the silk fibroin latex spread evenly in the area. The ambient temperature is about 28°C during painting; during the process of painting, the water in the silk fibroin latex gradually evaporates, and the milky white of the latex gradually recedes. When it basically disappears, the silk fibroin film on the PET low-viscosity film material has initially achieved molding. Next, gently paste the treated silk support material on the surface of the silk film in the working area, and use a rubber roller to evenly roll on the silk support material. The hardness of the surface of the rubber roller is between 70-75. The average pressure of rolling is 15-20kg. Repeat the rolling operation until it is smooth and even. Due to the difference in adhesive stress between the silk scaffold material and the PET low-adhesive film material, the silk scaffold material is adhered to the silk scaffold material evenly and completely after the silk scaffold material is peeled off from the PET low-viscosity film material. The surface forms a reinforcement bracket. Place the silk pattern to be reinforced flat on a smooth flat surface, with the reverse facing up, and fix it with pressure strips around it. The side of the reinforced bracket with the silk film is gently pressed to the reverse side of the silk pattern, and rolled and pressed with a rubber roller. The hardness of the surface of the rubber roller is between 70-75, and the average pressure is 15- 20kg. After the pressing is even and uniform, move the reinforced silk pattern on a flat workbench for 24 hours of balance, and the balance temperature is room temperature;

D、放置丝绸纹样:打开防雾罩2,将支架加固处理后的丝绸纹样平放在处理箱1中的网状处理架6上,正面朝上,盖上处理箱防雾罩2;D. Place the silk pattern: open the anti-fog cover 2, place the silk pattern after the bracket reinforcement treatment on the mesh processing frame 6 in the processing box 1, face up, and cover the anti-fog cover 2 of the processing box;

E、喷雾处理:喷雾时喷雾装置8的转速为20—40转/分,处理液的用量根据纹样的织物特点、结构以及保护的具体要求,由处理液用量控制器10进行控制,一般用量在150—350ml/m2内;E, spray treatment: during spraying, the rotating speed of spray device 8 is 20-40 rpm, and the consumption of treatment liquid is controlled by treatment liquid consumption controller 10 according to the fabric characteristics, structure and protection specific requirements of patterns. 150—350ml/ m2 ;

F、吸风处理:喷雾完成后,打开防雾罩2,在丝绸纹样上放上压框7,然后进行吸风处理,这时,纹样需对准网状处理架6上的丝网部分,压框7压上时保证纹样的四周正好压住纹样,在吸风过程中防止纹样移动,吸风以微风方式进行,主要是促使纹样表面的处理液能向纹样内部进行渗透,吸风量一般控制在0.5—1.5m3/h之间,吸风时间控制在60—120分钟;F, suction treatment: after the spraying is completed, open the anti-fog cover 2, put the pressure frame 7 on the silk pattern, and then carry out the suction treatment. At this time, the pattern needs to be aligned with the silk screen part on the mesh processing frame 6, When the pressure frame 7 is pressed, ensure that the surroundings of the pattern just press the pattern, and prevent the pattern from moving during the suction process. The suction is carried out in a breeze, mainly to promote the treatment liquid on the surface of the pattern to penetrate into the interior of the pattern, and the air suction volume is generally controlled. Between 0.5-1.5m 3 /h, the suction time is controlled at 60-120 minutes;

G、干燥处理:开启红外干燥器3进行干燥,干燥温度一般在35—60℃之间,时间为20—40分钟;G. Drying treatment: turn on the infrared dryer 3 to dry, the drying temperature is generally between 35-60°C, and the time is 20-40 minutes;

H、将经过干燥处理后的丝绸纹样,进行自然平衡24h,完成对丝绸纹样的非接触式处理。H. Naturally balance the dried silk pattern for 24 hours to complete the non-contact processing of the silk pattern.

具体实施例一:Specific embodiment one:

1、用去离子水按以下成份、配比配制防霉处理液备用:FM-2598-1防霉剂:5 wt%;丝素粉:2 wt%;溶剂: 去离子水;1. Use deionized water to prepare anti-mold treatment solution according to the following ingredients and ratios: FM-2598-1 anti-mold agent: 5 wt%; silk fibroin powder: 2 wt%; solvent: deionized water;

2、将织物重量为26克/平方米的真丝纺作为加固的丝绸支架材料,浸入防霉处理液内进行处理。待充分湿润后取出,放在平板上用橡胶滚筒进行正反面的滚轧操作。经二浸二轧处理后,自然干燥备用。2. The silk spun with a fabric weight of 26 grams per square meter is used as a reinforced silk support material, and is immersed in the anti-mildew treatment solution for processing. Take it out after it is fully wet, put it on a flat plate and use a rubber roller to roll the front and back sides. After two dipping and two rolling treatments, it is naturally dried for later use.

3、按以下成份配比对丝素胶乳液进行配制:3. Prepare silk fibroin latex according to the following composition ratio:

丙烯酸聚合物乳液:40wt%;丝素粉:2wt%;溶剂:去离子水;Acrylic polymer emulsion: 40wt%; silk fibroin powder: 2wt%; solvent: deionized water;

所述丙烯酸聚合物乳液中各单体的重量比例为:甲基丙烯酸甲酯:13%;丙烯酸丁酯:78%;丙烯酸:5%;丙烯酸-2-羟乙酯:4%The weight ratio of each monomer in the acrylic acid polymer emulsion is: methyl methacrylate: 13%; butyl acrylate: 78%; acrylic acid: 5%; 2-hydroxyethyl acrylate: 4%

4、在PET低粘性薄膜材料表面设置25×34cm的支架制作工作区域,在该区域内均匀涂覆制备的以上丝素胶乳液,乳液用量为8ml。具体操作步骤为:用一次性注射器吸取8mL丝素胶乳液,均匀滴到低粘性薄膜材料工作区域内,用毛长约10mm的羊毫毛刷,在工作区域内对乳液进行横向和纵向的反复涂刷,使丝素胶乳液在区域内分布均匀,涂刷时的环境温度为28℃左右。在涂刷过程中,丝素胶乳液中的水分逐步蒸发,乳液的乳白色逐步退去。待乳白色基本消失时,将经浸轧处理的真丝纺轻轻地粘贴到工作区域内的丝素胶膜表面,用橡胶滚筒在真丝纺上均匀地进行滚压,橡胶滚筒表面的硬度为72度,滚压的平均压力为15kg。反复滚压操作,直到平整均匀。同时把需加固处理的丝绸古香缎纹样平放在光滑的平板表面,反面朝上,四周用压条固定。丝绸古香缎纹样,尺寸为:20×30cm,重量为:158克/平方米。这时将真丝纺从PET低粘性薄膜材料上进行剥离,同时将其带丝素胶膜的一面轻轻地压覆到丝绸古香缎纹样的反面,用橡胶滚筒进行滚动加压,橡胶硬度同上,平均加压压力为 15kg。压覆平整均匀后将加固后的丝绸古香缎纹样移置平整的工作台上进行24h的平衡,平衡温度为常温。4. On the surface of PET low-viscosity film material, set up a work area of 25×34 cm for stent making, and evenly coat the above prepared silk fibroin glue emulsion in this area, and the amount of emulsion is 8ml. The specific operation steps are: use a disposable syringe to absorb 8mL silk fibroin glue emulsion, evenly drop it into the working area of the low-viscosity film material, use a wool brush with a hair length of about 10mm, and repeatedly apply the emulsion horizontally and vertically in the working area Brush to make the silk fibroin latex evenly distributed in the area, and the ambient temperature when brushing is about 28°C. During the painting process, the water in the silk fibroin latex evaporates gradually, and the milky white of the emulsion fades away gradually. When the milky white color basically disappears, gently paste the padded real silk on the surface of the silk fibroin film in the working area, and roll it evenly on the real silk with a rubber roller. The hardness of the rubber roller surface is 72 degrees. , The average rolling pressure is 15kg. Repeat the rolling operation until it is smooth and even. At the same time, put the silk antique satin pattern that needs to be reinforced on a smooth flat surface, with the reverse side facing up, and fix it with pressing strips around it. Silk antique satin pattern, size: 20×30cm, weight: 158g/square meter. At this time, the silk fabric is peeled off from the PET low-viscosity film material, and at the same time, the side with the silk film is gently pressed onto the reverse side of the silk antique satin pattern, and the rubber roller is used for rolling and pressing, and the rubber hardness is the same as above. , The average pressurized pressure is 15kg. After the pressing is even and uniform, the reinforced silk antique satin pattern is moved to a flat workbench for 24 hours of balance, and the balance temperature is room temperature.

5、纹样经平衡后,打开防雾罩2,将加固后的丝绸古香缎纹样平放在处理箱1中的网状处理架6上,对准丝网部分,正面朝上,盖上处理箱防雾罩2,用防霉处理液在加固后的丝绸古香缎纹样的正面进行喷雾处理。喷雾时喷雾装置8转速为25转/分,处理液用量为250ml/m2。喷雾完成后,打开防雾罩2,放上压框7进行吸风处理,吸风量控制在1.0m3/h左右,吸风时间为120分钟。吸风完成后,开启红外干燥器3进行干燥,干燥温度一般在50℃,时间为20分钟。处理完成后,放入另一丝网架上进行自然平衡24h。5. After the pattern is balanced, open the anti-fog cover 2, place the reinforced silk antique satin pattern on the mesh processing frame 6 in the processing box 1, align it with the silk screen, face up, and cover it for processing Box anti-fog cover 2, carry out spray processing with anti-mildew treatment liquid on the front of the silk antique satin pattern pattern after reinforcement. When spraying, the rotational speed of the spray device 8 is 25 rpm, and the dosage of the treatment liquid is 250ml/m 2 . After the spraying is completed, open the anti-fog cover 2, put on the pressure frame 7 to carry out air suction treatment, the air suction volume is controlled at about 1.0m 3 /h, and the air suction time is 120 minutes. After the suction is completed, the infrared dryer 3 is turned on for drying. The drying temperature is generally 50° C. for 20 minutes. After the treatment is completed, put it into another wire mesh rack for natural balance for 24 hours.

6、对处理后的丝绸古香缎纹样进行殖菌培养,观察试样表面真菌生长情况,实验菌株为黑曲霉(Aspergillus niger),试验温度:28℃;时间:7天;相对湿度RH≥ 95%。实验结果为“肉眼观察,未见霉菌生长”,表明该非接触式处理方法能起到良好的防腐效果,避免接触式处理对丝绸古香缎纹样的破坏。 6. Carry out bacterial culture on the treated silk antique satin pattern, observe the growth of fungi on the surface of the sample, the experimental strain is Aspergillus niger, test temperature: 28°C; time: 7 days; relative humidity RH ≥ 95 %. The result of the experiment was "no mold growth was observed with the naked eye", indicating that the non-contact treatment method can have a good antiseptic effect and avoid the damage to the ancient satin pattern of silk by contact treatment.

上述实施例只为说明本发明的技术构思及特点,其目的在于让熟悉此项技术的人士能够了解本发明的内容并加以实施,并不能以此限制本发明的保护范围,凡根据本发明精神实质所作的等效变化或修饰,都应涵盖在本发明的保护范围内。The above-mentioned embodiments are only to illustrate the technical conception and characteristics of the present invention, and its purpose is to allow those familiar with this technology to understand the content of the present invention and implement it, and cannot limit the protection scope of the present invention with this. Substantial equivalent changes or modifications shall fall within the protection scope of the present invention.

Claims (6)

1. a kind of contactless processing unit of Silk pattern, it is characterised in that:Including treatment box and demister screen;The treatment box Internal bottom surface is provided with infrared heater;The bottom of the treatment box is provided with inlet scoop;The inlet scoop connects air suction device; Top inside the treatment box is provided with support frame;Net-shape processed frame is provided with support frame as described above;The net-shape processed frame On be provided with press box;The upper end of the treatment box is provided with demister screen;Upper end inside the demister screen is provided with sprayer unit; One end connection transfusion pole of the sprayer unit;Liquid amount controller is provided with the transfusion pole;The liquid amount controller The outer miniature force (forcing) pump of company;The spraying, which is loaded onto, is provided with fog-spray nozzle;The sprayer unit rotates around transfusion pole.
2. a kind of contactless processing unit of Silk pattern according to claim 1, it is characterised in that:The inlet scoop Treatment box is distributed in all around on four sides;Inlet scoop at least six.
3. a kind of contactless processing unit of Silk pattern according to claim 1, it is characterised in that:The spraying dress Put including four injection spray pipes parallel with transfusion pole;Four injection spray pipes are distributed in the orientation of the upper and lower, left and right of transfusion pole;Institute Fog-spray nozzle is stated to be uniformly distributed on injection spray pipe;At least six fog-spray nozzles on every injection spray pipe.
4. a kind of contactless processing unit of Silk pattern according to claim 1, it is characterised in that:The netted place The silk screen of reason frame is worn into twisting nylon yarn.
5. a kind of contactless processing unit of Silk pattern according to claim 1, it is characterised in that:The press box Inside and outside size is identical with the interior outside dimension that silk screen handles frame.
6. a kind of contactless processing method of Silk pattern, it is characterised in that:Comprise the following steps:
1)Prepare treatment fluid:With deionized water mould proof or anti-light treatment fluid is prepared by following composition, proportioning;
Mould proof treatment fluid:Mould inhibitor:1-5 wt%;Fibroin powder:1-8 wt%:Solvent:Deionized water;
Anti-light treatment fluid:Light stability agent:5-15 wt%;Fibroin powder:1-8 wt%;Solvent:Deionized water;
2) handle the Silk pattern reinforced without support using the contactless processing unit of Silk pattern or need first support to reinforce Silk pattern;
The specific steps for the Silk pattern that the contactless processing unit processing of the use Silk pattern is reinforced without support are such as Under:
A, placement Silk pattern:Silk pattern is lain on the net-shape processed frame in treatment box, reverse side is upward;
B, spraying treatment:Reverse side with the treatment fluid configured in Silk pattern carries out spraying treatment;Sprayer unit during spraying Rotating speed is 20-40 revs/min, is controlled by treatment fluid with amount controller, and general liquid consumption control is in 150-350ml/m2;
C, air draught processing:After the completion of spraying, press box is pressed on net-shape processed frame, and air draught is carried out in gentle breeze mode, and suction air volume is general Control is between 0.5-1.5m3/h, and air draught time control was at 60-120 minutes;
D, drying process:After the completion of air draught, open infrared dryer be dried, drying temperature typically between 35-60 DEG C, Time is 20-40 minutes;
E, Silk pattern face-up placed, and carry out spraying treatment, air draught processing, drying process successively;
F, the positive and negative of Silk pattern have all carried out to spraying treatment, air draught processing, drying process after, carry out natural equilibrium 24h;
The contactless processing unit processing of the use Silk pattern needs the specific steps of the Silk pattern of first support reinforcing such as Under:
A, reinforcement material processing:Silk timbering material is immersed in mould proof or anti-light treatment fluid, takes out, is placed on after being sufficiently humidified so as to The rolling operation of positive and negative is carried out on flat board with rubber cylinder;After treatment fluid " two leachings two are rolled ", natural drying is carried out standby;
B, preparation fibroin latex solution:Fibroin latex solution is prepared by following composition, proportioning:
Acrylate polymer emulsion:30-45 wt%;Fibroin powder:1-4 wt% solvents:Deionized water;
The weight ratio of each monomer is in the acrylate polymer emulsion:Methyl methacrylate:10-15 %, butyl acrylate: 75-85 %;Acrylic acid:3-7 %;Acrylic acid -2- hydroxyl ethyl esters:2-5 %;
C, support consolidation process:Support is set to make working region in the low adhesive membrane material surfaces of PET, in working region Even to coat the fibroin latex solution prepared, the consumption of fibroin latex solution is in 8-10ml;8-10mL are drawn with disposable syringe Plain latex solution, is uniformly dripped in the domain of low adhesive membrane material work area;Writing brush made of goat's hair hairbrush is used, emulsion is carried out in working region horizontal To the brushing repeatedly with longitudinal direction, fibroin latex solution is set to be evenly distributed in region, environment temperature during brushing is 27-29 DEG C; In painting process, during milky white decoloration in fibroin latex solution, the fibroin glued membrane on the low adhesive membrane materials of PET tentatively reaches Shaping;The silk timbering material that process pads processing is pasted to the fibroin film surface in working region, existed with rubber cylinder Rolled on silk timbering material, the hardness on rubber cylinder surface is 70-75, and rolling pressure is 15-20kg;By silk support After material is peeled off from the low adhesive membrane materials of PET, fibroin glued membrane is adhered to uniformly and intactly silk timbering material surface Form reinforced liner;The Silk pattern that needs reinforcement is lain in smooth planar surface, reverse side upward, with press strip fixed by surrounding; One side of the reinforced liner with fibroin glued membrane is covered to the reverse side of Silk pattern, blend rubber roller carries out rolling pressurization, rubber The hardness on glue cylinder surface is 70-75, and moulding pressure is 15-20kg;Cover the Silk pattern shifting after reinforcing after even uniform 24h balance is carried out on the whole workbench of horizontalization, equilibrium temperature is normal temperature;
D, placement Silk pattern:Silk pattern Jing Guo support consolidation process is lain on the net-shape processed frame in treatment box, Face-up;
E, spraying treatment:Reverse side with the treatment fluid configured in Silk pattern carries out spraying treatment;Sprayer unit during spraying Rotating speed is 20-40 revs/min, is controlled by treatment fluid with amount controller, and general liquid consumption control is in 150-350ml/m2It is interior;
F, air draught processing:After the completion of spraying, press box is pressed on net-shape processed frame, and air draught is carried out in gentle breeze mode, and suction air volume is general Control is in 0.5-1.5m3Between/h, air draught time control was at 60-120 minutes;
G, drying process:After the completion of air draught, open infrared dryer be dried, drying temperature typically between 35-60 DEG C, Time is 20-40 minutes;
H, by the Silk pattern after drying process, carry out natural equilibrium 24h.
CN201710377381.9A 2017-05-25 2017-05-25 A non-contact processing device and method for silk patterns Active CN107059300B (en)