Detailed Description
The electrolyte and the secondary battery according to the present invention will be described in detail below.
First, the electrolytic solution according to the first aspect of the invention is explained.
The electrolyte solution according to the first aspect of the invention includes: electrolyte salt, organic solvent and additive. The organic solvent includes a carboxylic acid ester compound. The additive comprises cyclic sulfate and triphenyl phosphite.
In the electrolytic solution according to the first aspect of the invention, the carboxylate compound is used to improve the rate performance of the secondary battery, but when the carboxylate compound is applied to a secondary battery of a high voltage system, it is easily decomposed by oxidation, and in addition, when the secondary battery using the carboxylate compound is used under a high temperature environment, the capacity loss of the secondary battery after many cycles is serious, and the high temperature storage performance of the secondary battery is seriously deteriorated. The cyclic sulfate has a high reduction potential, and can preferentially form a film on the surface of the negative electrode to inhibit the reduction of the carboxylate compound, thereby improving the cycle performance of the secondary battery. Triphenyl phosphite can react with HF, and the effect of reducing HF is achieved, so that the high-temperature storage performance of the secondary battery is improved. When the electrolyte contains three substances, the rate capability, the cycle performance and the storage performance of the secondary battery under high temperature and high voltage can be improved simultaneously under the synergistic effect of the three substances.
In the electrolyte according to the first aspect of the present invention, the carboxylate compound is one or more selected from compounds represented by formula i. Wherein R is1、R2Each independently selected from one of C1-10 alkyl and C1-10 halogenated alkyl; halogenatedThe halogen atom in the alkyl is selected from one or more of F, Cl, Br and I.
In the electrolyte according to the first aspect of the present invention, the alkyl group having 1 to 10 carbon atoms may be a chain alkyl group or a cyclic alkyl group. Among them, the chain alkyl group includes a straight chain alkyl group and a branched chain alkyl group. The cyclic alkyl group may or may not have a substituent. In the above-mentioned alkyl group, the lower limit of the number of carbon atoms may be preferably 1,2 or 3, and the upper limit of the number of carbon atoms may be preferably 4, 5, 6, 7, 8 or 10. Preferably, R1、R2Each independently selected from a chain alkyl group having 1 to 6 carbon atoms or a cyclic alkyl group having 3 to 8 carbon atoms. Even more preferably, R1、R2Each independently selected from a chain alkyl group having 1 to 4 carbon atoms or a cyclic alkyl group having 5 to 7 carbon atoms.
Specifically, the alkyl group having 1 to 10 carbon atoms may be one selected from the group consisting of a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a cyclopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a cyclobutyl group, a n-pentyl group, an isopentyl group, a tert-pentyl group, a neopentyl group, a cyclopentyl group, a2, 2-dimethylpropyl group, a 1-ethylpropyl group, a 1-methylbutyl group, a 2-methylbutyl group, a n-hexyl group, an isohexyl group, a 2-hexyl group, a 3-hexyl group, a cyclohexyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 1,1, 2-trimethylpropyl group, a 3, 3-dimethylbutyl group, a n-heptyl group, a 2-heptyl group, a 3-heptyl group, a 2-methylhexyl group, a 3-.
In the electrolyte solution according to the first aspect of the present invention, the number of substitution of halogen atoms in the halogenated alkyl group having 1 to 10 carbon atoms and the substitution position thereof are not particularly limited and may be selected according to actual needs. Specifically, the number of halogen atoms may be 1,2, 3 or 4. When having halogen atomsWhen the number is 2 or more, the halogen atoms may be the same, may be completely different, or may be partially the same. The alkyl halide may be a chain alkyl halide or a cyclic alkyl halide. The chain halogenated alkyl groups further include straight chain halogenated alkyl groups and branched chain halogenated alkyl groups. The cyclic alkyl halide group may or may not have a substituent. In the haloalkane group, the number of carbon atoms may be preferably lower than 1,2 or 3, and the number of carbon atoms may be preferably upper than 4, 5, 6, 7, 8 or 10. Preferably, R1、R2Each independently selected from a chain alkyl halide having 1 to 6 carbon atoms or a cyclic alkyl halide having 3 to 8 carbon atoms. Even more preferably, R1、R2Each independently selected from a chain alkyl halide having 1 to 4 carbon atoms or a cyclic alkyl halide having 5 to 7 carbon atoms.
Specifically, the alkyl halide having 1 to 10 carbon atoms is selected from the group consisting of chloromethyl, dichloromethyl, trichloromethyl, 1-chloroethyl, 1, 2-dichloroethyl, 2-chloro-n-propyl, 2-dichloro-n-propyl, 1-chloroisopropyl, monochloropropyl, 1-chloro-n-butyl, 2-chloroisobutyl, monochlorocyclobutyl, 1-chloro-n-pentyl, 2-chloro-n-pentyl, 1-chloroisopentyl, 2-dichloromethylpropyl, monochlorocyclopentyl, 3-chloro-2, 2-dimethylpropyl, 1-chloro-1-ethylpropyl, 1-chloro-1-methylbutyl, 2-chloro-2-methylbutyl, 2-chloro-n-hexyl, monochlorocyclohexyl, 2-chloromethylpentyl, chlorocyclohexyl, chlorocyclopentyl, chlorobutyl, 3-chloro-3-methylpentyl, 2-chloro-1, 1, 2-trimethylpropyl, 4-chloro-3, 3-dimethylbutyl, 2-chloro-n-heptyl. In the above groups, the Cl atom in the alkyl halide group can be partially or completely substituted by one or more of F, Br and I.
In the electrolyte according to the first aspect of the present invention, the carboxylate compound may be selected from one or more of methyl formate, ethyl acetate, ethyl propionate, ethyl valerate, ethyl isovalerate, propyl propionate, butyl propionate, isobutyl propionate, butyl butyrate, butyl isobutyrate, pentyl butyrate, isopentyl butyrate, pentyl propionate, isopentyl propionate, ethyl isopropionate, ethyl butyrate, ethyl isobutyrate, propyl valerate, propyl isovalerate, ethyl isovalerate, and compounds in which the specific carboxylate compound is partially or fully substituted with one or more of F, Cl, Br, and I.
In the electrolyte according to the first aspect of the present invention, the cyclic sulfate is selected from one or more compounds represented by formula ii. Wherein n is an integer within 1-3; r3、R4、R5、R6Each independently selected from one of H, F, Cl, Br, I, alkyl with 1-10 carbon atoms and alkoxy with 1-10 carbon atoms, wherein H on the alkyl and the alkoxy can be substituted by one or more of F, Cl, Br and I.
In the electrolyte according to the first aspect of the present invention, specifically, the cyclic sulfate is selected from one or more of the following compounds;
in the electrolyte according to the first aspect of the present invention, the triphenyl phosphite has the following structure:
in the electrolytic solution according to the first aspect of the invention, the volume of the carboxylate compound is 5% to 50% of the total volume of the organic solvent. Preferably, the volume of the carboxylate compound is 10% to 40% of the total volume of the organic solvent. Further preferably, the volume of the carboxylate compound is 20% to 35% of the total volume of the organic solvent.
In the electrolyte according to the first aspect of the present invention, the content of the cyclic sulfate is 0.5% to 10% by weight of the total weight of the electrolyte. Preferably, the content of the cyclic sulfate is 1 to 5% of the total weight of the electrolyte.
In the electrolyte according to the first aspect of the present invention, the content of triphenyl phosphite is 0.03% to 1% of the total weight of the electrolyte. Preferably, the content of the triphenyl phosphite is 0.1-0.3% of the total weight of the electrolyte.
In the electrolyte according to the first aspect of the present invention, the specific type of the organic solvent is not particularly limited, and may be selected according to actual needs. Preferably, a non-aqueous organic solvent is used. The organic solvent may also include any kind of carbonates and halogenated compounds of carbonates. The carbonate includes cyclic carbonate and chain carbonate. Specifically, the organic solvent may further include one or more of Ethylene Carbonate (EC), Propylene Carbonate (PC), butylene carbonate, pentylene carbonate, fluoroethylene carbonate, dimethyl carbonate, diethyl carbonate (DEC), dipropyl carbonate, methylethyl carbonate, γ -butyrolactone, and tetrahydrofuran.
In the electrolytic solution according to the first aspect of the invention, the electrolyte salt may be selected from a lithium salt, a sodium salt, or a zinc salt, depending on the secondary battery to which the electrolytic solution is applied.
In the electrolytic solution according to the first aspect of the invention, the content of the electrolyte salt is 6.2% to 25% by weight of the total weight of the electrolytic solution. Preferably, the content of the electrolyte salt is 6.25 to 18.8% of the total weight of the electrolyte. Further preferably, the content of the electrolyte salt is 10% to 15% of the total weight of the electrolyte.
The electrolyte is prepared by adopting a conventional method, namely, all materials in the electrolyte are uniformly mixed.
Next, a secondary battery according to a second aspect of the invention is explained.
A secondary battery according to a second aspect of the invention includes the electrolyte according to the first aspect of the invention.
In the secondary battery according to the second aspect of the invention, the secondary battery further includes a positive electrode tab, a negative electrode tab, and a separator.
In the secondary battery according to the second aspect of the invention, the positive electrode sheet includes a positive electrode current collector and a positive electrode active slurry layer on the positive electrode current collector, wherein the positive electrode active slurry layer includes a positive electrode active material. The specific type of the positive electrode active material is not particularly limited, and may be selected according to the requirement.
In the secondary battery according to the second aspect of the invention, the negative electrode tab includes a negative electrode current collector and a negative electrode active slurry layer on the negative electrode current collector. The negative active paste layer includes a negative active material. The specific type of the negative active material is not particularly limited, and may be selected as needed.
In the secondary battery according to the second aspect of the present invention, the specific kind of the separator is not particularly limited and may be any separator material used in the existing secondary battery, such as polyethylene, polypropylene, polyvinylidene fluoride, and multilayer composite films thereof, but is not limited thereto.
In the secondary battery according to the second aspect of the invention, the secondary battery may be a lithium ion secondary battery, a sodium ion secondary battery, or a zinc ion secondary battery.
When the secondary battery is a lithium ion secondary battery, preferably, the positive electrode active material is selected from lithium cobaltate (LiCoO)2) Lithium nickelate (LiNiO)2) Olivine-type lithium iron phosphate (LiFePO)4) Olivine type LiMPO4Spinel type LiMn2O4Ternary positive electrode material LiNixAyB(1-x-y)O2And Li1-x’(A’y’B’z’C1-y’-z’)O2One or more of them. Wherein M is selected from one or more of Co, Ni, Fe, Mn and V; A. b is independently selected from one of Co, Al and Mn, and A and B are different; 0<x<1,0<y<1 and x + y<1;0≤x’<1,0≤y’<1,0≤z’<1 and y '+ z'<1; a ', B' and C are respectively and independently selected from one of Co, Ni, Fe and Mn, and A ', B' and C are different. The negative active material may be selected from metallic lithium, and the negative active material may also be selected from lithium/lithium+A material capable of intercalating lithium when the electrode potential of the equilibrium potential is < 2V. Specifically, the negative active material is selected from natural graphite, artificial graphite, mesophase micro carbon spheres (abbreviated as MCMB), hard carbon, soft carbon, silicon-carbon composite, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO2Spinel-structured lithiated TiO2-Li4Ti5O12And one or more of Li-Al alloy. The electrolyte salt may be a lithium salt, which may be selected from LiPF6、LiBF4、LiN(SO2F)2(abbreviated LiFSI), LiN (CF)3SO2)2(abbreviated as LiTFSi), LiClO4、LiAsF6、LiB(C2O4)2(abbreviated as LiBOB) and LiBF2C2O4(abbreviated as LiDFOB) LiPO2F2One or more of them.
The present application is further illustrated below with reference to examples. It should be understood that these examples are for illustrative purposes only and are not intended to limit the scope of the present application. In the embodiment, only the case where the secondary battery is a lithium ion secondary battery is shown, but the present invention is not limited thereto.
In the following examples, reagents, materials and instruments used are commercially available unless otherwise specified.
The lithium ion secondary batteries of examples 1 to 11 and comparative examples 1 to 7 were each prepared as follows.
(1) Preparation of positive plate
The positive electrode active material lithium cobaltate (LiCoO)2) Mixing polyvinylidene fluoride serving as a binder and acetylene black serving as a conductive agent according to a weight ratio of 98:1:1, adding N-methyl pyrrolidone (NMP), and stirring under the action of a vacuum stirrer until the system becomes uniform and transparent to obtain anode slurry; uniformly coating the positive electrode slurry on a positive electrode current collector aluminum foil with the thickness of 12 mu m; and (3) airing the aluminum foil at room temperature, transferring the aluminum foil to a 120 ℃ oven for drying for 1h, and then performing cold pressing and slitting to obtain the positive plate.
(2) Preparation of negative plate
Mixing the artificial graphite serving as the negative electrode active material, sodium carboxymethyl cellulose (CMC) serving as a thickening agent and styrene butadiene rubber serving as a binder according to the weight ratio of 98:1:1, adding deionized water, and obtaining negative electrode slurry under the action of a vacuum stirrer; uniformly coating the negative electrode slurry on a negative electrode current collector copper foil with the thickness of 8 mu m; and (3) airing the copper foil at room temperature, transferring the copper foil to a 120 ℃ oven for drying for 1h, and then performing cold pressing and slitting to obtain the negative plate.
(3) Preparation of electrolyte
At water content<In a 10ppm argon atmosphere glove box, EC, PC, DEC were mixed at a volume ratio of EC: PC: DEC of 1:1:1, followed by a fully dried lithium salt LiPF6Dissolving in a mixed organic solvent, adding a carboxylic ester compound, cyclic sulfate and triphenyl phosphite, and uniformly mixing to obtain the electrolyte. Wherein, LiPF6The content of (b) was 12.5% by weight of the total electrolyte. Specific kinds and contents of the carboxylate compound, cyclic sulfate ester and triphenyl phosphite used in the electrolyte are shown in table 1. In Table 1, the content of the carboxylate compound is a volume percentage calculated based on the total volume of the organic solvent, cyclic sulfate ester and triphenyl phosphiteThe content of the ester is a weight percentage calculated based on the total weight of the electrolyte.
(4) Preparation of the separator
A16 μm thick polypropylene separator (model A273 from Celgard) was used.
(5) Preparation of lithium ion secondary battery
Stacking the positive plate, the isolating film and the negative plate in sequence to enable the isolating film to be positioned between the positive plate and the negative plate to play an isolating role, and then winding to obtain a bare cell; and placing the bare cell in an outer packaging foil, injecting the prepared electrolyte into the dried bare cell, and performing vacuum packaging, standing, formation, shaping and other processes to obtain the lithium ion secondary battery.
Next, a test procedure of the lithium ion secondary battery is explained.
(1) Rate capability test of lithium ion secondary battery
The lithium ion secondary battery was charged at a constant current of 1C (nominal capacity) to a voltage of 4.4V at 25C, then charged at a constant voltage of 4.4V to a current of 0.05C or less, left for 5min, and then discharged at a constant current of 0.2C to a cut-off voltage of 3V, at which the discharge capacity was recorded as D0.
And then charging the lithium ion secondary battery to a voltage of 4.4V at a constant current of 1C, then charging to a current of less than or equal to 0.05C at a constant voltage of 4.4V, standing for 5min, and then discharging to a cut-off voltage of 3V at a constant current of 2C, wherein the discharge capacity at the moment is recorded as D1.
The lithium ion secondary battery 2C/0.2C rate performance is D1/D0 × 100%.
(2) High temperature cycle performance test of lithium ion secondary battery
At 45 ℃, the lithium ion secondary battery is charged at a constant current of 1C until the voltage is 4.4V, further charged at a constant voltage of 4.4V until the current is 0.05C, and then discharged at a constant current of 1C until the voltage is 3.0V, which is a charge-discharge cycle process, and the discharge capacity of the time is the discharge capacity of the first cycle. The lithium ion secondary battery was subjected to 300-cycle charge/discharge tests in accordance with the above-described method, and the discharge capacity at the 300 th cycle was detected.
Capacity retention (%) after the lithium ion secondary battery was cycled 300 times ═ 100% (discharge capacity of the lithium ion secondary battery cycled 300 times/discharge capacity of the lithium ion secondary battery cycled for the first time).
(3) High temperature storage performance test of lithium ion secondary battery
The lithium ion secondary battery was charged at 85 ℃ to a voltage of 4.4V at a constant current of 0.5C and then charged at a constant voltage of 4.4V to a current of 0.05C, at which time the thickness of the lithium ion secondary battery was measured and recorded as h0(ii) a Then the lithium ion secondary battery is placed into a thermostat with the temperature of 85 ℃, stored for 24 hours and taken out, the thickness of the lithium ion secondary battery at the moment is tested and recorded as h1。
Thickness expansion rate (%) of the lithium ion secondary battery after 24 hours of storage1-h0)/h0]×100%。
Table 1 shows the parameters and performance test results for examples 1-11 and comparative examples 1-7.
As can be seen from the analysis of the relevant data in table 1, the carboxylate compound, the cyclic phosphate and the triphenyl phosphite are not added in comparative example 1, and the rate capability, the high-temperature cycle performance and the high-temperature storage performance of the lithium ion secondary battery are poor; when only the carboxylate compound was contained in the electrolyte (comparative example 2), the rate performance of the lithium ion secondary battery was improved, but the high-temperature cycle performance and the high-temperature storage performance were deteriorated; when the electrolyte only contains the cyclic sulfate (comparative example 3), the high-temperature cycle performance of the lithium ion secondary battery is improved, and the rate performance and the high-temperature storage performance are not obviously changed; when only triphenyl phosphite was contained in the electrolyte (comparative example 4), the high-temperature storage performance of the lithium ion secondary battery was improved, but the rate performance was deteriorated; when a carboxylate compound and a cyclic sulfate ester were added to the electrolyte at the same time (comparative example 5), the high-temperature cycle performance could be improved while the rate performance was improved, but the high-temperature storage performance was seriously deteriorated. When the carboxylate compound and triphenyl phosphite are added into the electrolyte (comparative example 6), the rate capability and the high-temperature storage capability can be considered, but the high-temperature cycle performance is deteriorated; when cyclic sulfate and triphenyl phosphite were added to the electrolyte at the same time (comparative example 7), the high-temperature cycle performance and the high-temperature storage performance could be improved, but the rate performance appeared to be deteriorated.
When the electrolyte contains the carboxylate compound, the cyclic phosphate and the triphenyl phosphite, the lithium ion secondary battery has better rate performance and better high-temperature cycle performance and high-temperature storage performance.
Those skilled in the art to which the present application pertains can also make appropriate changes and modifications to the above-described embodiments, based on the disclosure of the above description. Therefore, the present application is not limited to the specific embodiments disclosed and described above, and some modifications and variations of the present application should fall within the scope of the claims of the present application.