CN110257924A - A kind of manufacture craft of gold silk foster skin quilt - Google Patents

A kind of manufacture craft of gold silk foster skin quilt Download PDF

Info

Publication number
CN110257924A
CN110257924A CN201910693798.5A CN201910693798A CN110257924A CN 110257924 A CN110257924 A CN 110257924A CN 201910693798 A CN201910693798 A CN 201910693798A CN 110257924 A CN110257924 A CN 110257924A
Authority
CN
China
Prior art keywords
cocoon
silk
layer
gold
water
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201910693798.5A
Other languages
Chinese (zh)
Inventor
林燕飞
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Jiangsu Tiefan Silk Science And Technology Creative Park Co Ltd
Original Assignee
Jiangsu Tiefan Silk Science And Technology Creative Park Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jiangsu Tiefan Silk Science And Technology Creative Park Co Ltd filed Critical Jiangsu Tiefan Silk Science And Technology Creative Park Co Ltd
Priority to CN201910693798.5A priority Critical patent/CN110257924A/en
Publication of CN110257924A publication Critical patent/CN110257924A/en
Pending legal-status Critical Current

Abstract

The invention discloses a kind of manufacture crafts of gold silk foster skin quilt, and in particular to articles for daily use manufacture field, including select silkworm, impregnate, permeating, boiling, adjustment, degreasing, dial cocoon, open and dial, clear drift, draw and core detecting step.The present invention passes through dipping, infiltration, the technique of boiling and adjustment carries out cocoon cooking to gold cocoon, it can guarantee the length and toughness of later period silk, and it can guarantee that the infiltration of silk cocoon is abundant, and shorten degreasing duration, it can avoid corrosion impact glossiness and smooth degree of the gold filament length time by skimmed milk, and the mode that drawing process is drawn using four people, using " full width plane net changes " technique, core paths crisscross footpaths between fields are fixed layer by layer, to reach 20 years technological effects for exempting to turn over, this guarantees the silk uniformity and service life of the various aspects of whole quilt, effectively avoid the displacement of comforter batt, guarantee the service life of silk quilt.

Description

A kind of manufacture craft of gold silk foster skin quilt
Technical field
The present invention relates to articles for daily use manufacture field, it is more particularly related to a kind of gold silk foster skin quilt Manufacture craft.
Background technique
In Japan, spun gold silkworm is seen as born insect, is from " present of sky ".Gold silk is also known as tribute silkworm, produces per year Amount is very rare, is the hired product of imperial family, India in ancient times, for weaving luxurious waistband and Sha Li (SAREE).Gold cocoon is Why the cocoon formed by spun gold silkworm, spun gold silkworm can spue golden silk, be is determined by gene, without any dyeing Agent, spun gold silkworm belong to the primary kind of nature, and product is very rare, and total output only accounts for whole world cocoon yield 0.0001%, so extremely precious.Gold silk possesses unique golden yellow, and bright color, quality is soft and smooth, and strong sandstorm is good, moisture absorption Property it is strong, glossiness is good, nowadays then becomes the states such as America and Europe, Japan and manufactures the raw material that top finery and bedding are liked.So using yellow Spun gold makes core, can bring many benefits to user.
Existing silk core uses artificial and machinery production two ways in the production process, although machinery production can mention High production speed, but final product quality is relatively relatively low, has impurity pore or small rib strip, and existing artificial production mechanism workmanship The core flexibility and service life that skill is produced are lower, easily deform, influence continuing to use for user.
Summary of the invention
In order to overcome the drawbacks described above of the prior art, the embodiment of the present invention provides a kind of production of gold silk foster skin quilt Technique carries out cocoon cooking to gold cocoon by dipping, infiltration, boiling and the technique of adjustment, it is ensured that the length of later period silk and tough Property degree, and can guarantee that the infiltration of silk cocoon is abundant, and shorten degreasing duration, can avoid corrosion of the gold filament length time by skimmed milk Glossiness and smooth degree are influenced, guarantees its service life, the mode that drawing process is drawn using four people, using " full width plane Net changes " technique, core paths crisscross footpaths between fields are fixed layer by layer, to reach 20 years technological effects for exempting to turn over, this guarantees each of whole quilt The silk uniformity and service life of aspect, effectively avoid the displacement of comforter batt, guarantee the service life of silk quilt.
To achieve the above object, the invention provides the following technical scheme: a kind of manufacture craft of gold silk foster skin quilt, institute State that specific step is as follows:
A) it selects silkworm: selecting without obvious damaged or slight crack spun gold silkworm silk cocoon;
B) cocoon cooking:
1. dipping: cocoon being immersed in warm water, cocoon layer is made to seep profit, and makes to tie water membrane outside cocoon layer, to enhance water flowing Can, it improves to resist and boils ability;
2. infiltration: using temperature difference permeating method, silk cocoon is first put into steaming part for permeation, carry out steam and cocoon chamber air Displacement, then moves to cocoon in about 60 DEG C of water at low temperature, because temperature declines, the intracavitary steam of cocoon and air to the cold after sharply receive Contracting keeps the intracavitary external pressure of cocoon different, achievees the purpose that cocoon layer seeps profit;
3. boiling: carrying out boiling to the cocoon for having seeped profit, main function is to make cocoon chamber guttation and cooked cocoon layer, i.e. raising cocoon layer The temperature of middle water, enters hydrone inside silk gum, increases silk gum volume, softens its swelling, while utilizing hot soup dissolution one Part silk gum;
4. adjustment: the cocoon of boiling first handled in warm water before cocoon out, and solidified outer layer silk gum slightly, to protect cocoon Cocoon, should be placed in after cocoon in about 50 DEG C of water temperature of cocoon bucket, water is about 1.5 times of silkworm cocoon volume by layer out;
C) silk cocoon after cocoon cooking degreasing: is put into 80 DEG C of soda bath;
D) it dials cocoon: the silk cocoon after degreasing being carried out to dial cocoon by hand, silk cocoon is dialled one by one on hand, silkworm chrysalis and Qi Hei are plucked The husking of color;
E) it opens and dials: will dial and formed on model on the cotton after cocoon to it on such as arciform bamboo model, uniformly to be spread out to cloth The silk floss pocket (also known as cotton cap) of arc-shaped;
F) clear drift: ready-made silk floss pocket is de- dry using clear water immersion;
G) air dry: the silk floss pocket of Tuo Ganhou is dried, when shine to seventy percent it is dry after go to shady and cool region and carry out air dry;
H) it draws: in such a way that four people draw, " cap " being pulled into whole cup size, by four people while well layer by layer of having an effect Word laying fixes core paths crisscross footpaths between fields layer by layer using " full width plane net changes " technique;
I) core detects: being sampled detection to every group of core, and formulates " examining report ", to effective component, heavyweight Weaving method etc. is labeled.
In a preferred embodiment, warm water temperature is set as 50-70 DEG C in the impregnation technology, and when immersion is a length of About 2-4 minutes.
In a preferred embodiment, the digesting technoloy environment be set as steam pressure 0.8-1.0KG/cm2, Under conditions of 100 DEG C of temperature.
In a preferred embodiment, the temperature setting of warm water is 60 DEG C in the adjusting process, and handling duration is set It is set to 1-2 minutes.
In a preferred embodiment, described group of cocoon process carries out in clean circulating water, and large aperture is arranged Filter screen is filtered.
In a preferred embodiment, osmosizing portion temperature setting is 100 DEG C in the osmosis process, and steam pressure is 0.05 kg/m2
In a preferred embodiment, caustic soda and water ratio are 1.5 to 100 in the degreasing process, and impregnate 50- 60 minutes.
Technical effect and advantage of the invention:
1, the present invention carries out cocoon cooking to gold cocoon by dipping, infiltration, boiling and the technique of adjustment, it is ensured that later period silk Length and toughness, and can guarantee that the infiltration of silk cocoon is abundant, and shorten degreasing duration, can avoid the gold filament length time by de- The corrosion impact glossiness and smooth degree of cosmetics guarantee its service life, the transfer when silk screen pocket shines dry to seventy percent of air dry process Air dry is carried out to shady and cool position, it is ensured that the fiber and fibroin ingredient of silk are not damaged, and further ensure silk Service life, and the mode that drawing process is drawn using four people, using " full width plane net changes " technique, core paths crisscross footpaths between fields layer Layer is fixed, to reach 20 years technological effects for exempting to turn over, this guarantees the silk uniformity of the various aspects of whole quilt and uses the longevity Life, effectively avoids the displacement of comforter batt, guarantees the service life of silk quilt;
2, the present invention, can be by the silkworm chrysalis and its black on gold cocoon by carrying out in clean circulating water in group cocoon process Husking manually plucked, guarantee the presentation quality of subsequent core, during which flowing water takes away the husking of silkworm chrysalis and its black, And large aperture filter screen can obstruct silk cocoon, avoid the loss of raw material, gold silk is 29D denier, and white silkworm silk is 21D but Buddhist nun You, gold silk is thinner than platinum silk size, and the core cohesive force made of gold silk is stronger, more personal, warmth retention property is more preferable, but Although its silk quality is very thin, fiber is longer than common silk, and (stress intensity of gold silk is common silk to more flexible 2 times or so), gold silk itself has potent antibacterial, and it is anti-oxidant, it is rich in 18 kinds of amino acid, natural decomposition living radical balance Foster skin, while a large amount of sleep factors are discharged, relieving mental strain and helping sleep, gold silk brass pigment content is higher than white silk by 30%, class Hu trailing plants Foretell 34 times that cellulose content is white silk, possess and inhibit 5 kinds of antibacterial abilities such as Escherichia coli, is rich in aromatic amino acid, can inhale The ultraviolet light in 300hm is zoomed in, anti-oxidant-decomposable multiple activities free radical can generate maintaining skin to user, promote The effect of sleep.
Specific embodiment
Below in conjunction with the embodiment in the present invention, technical solution in the embodiment of the present invention is carried out clearly and completely Description, it is clear that described embodiments are only a part of the embodiments of the present invention, instead of all the embodiments.Based on this hair Embodiment in bright, every other implementation obtained by those of ordinary skill in the art without making creative efforts Example, shall fall within the protection scope of the present invention.
Embodiment 1:
The present invention provides a kind of manufacture crafts of gold silk foster skin quilt, and described specific step is as follows:
A) it selects silkworm: selecting without obvious damaged or slight crack spun gold silkworm silk cocoon;
B) cocoon cooking:
1. infiltration: using temperature difference permeating method, silk cocoon is first put into steaming part for permeation, osmosizing portion temperature is set in osmosis process 100 DEG C are set to, steam pressure is 0.05 kg/m2, steam and cocoon chamber air are replaced, cocoon is then moved to about 60 DEG C water at low temperature in, because temperature declines, the intracavitary steam of cocoon and air to the cold after sharply shrink, keep the intracavitary external pressure of cocoon different, Achieve the purpose that cocoon layer seeps profit;
2. boiling: carrying out boiling to the cocoon for having seeped profit, main function is to make cocoon chamber guttation and cooked cocoon layer, i.e. raising cocoon layer The temperature of middle water, enters hydrone inside silk gum, increases silk gum volume, softens its swelling, while utilizing hot soup dissolution one Part silk gum, digesting technoloy environment are set as under conditions of steam pressure 0.8-1.0KG/cm2,100 DEG C of temperature;
3. adjustment: the cocoon of boiling first handled in warm water before cocoon out, and solidified outer layer silk gum slightly, to protect cocoon Cocoon, should be placed in after cocoon in about 50 DEG C of water temperature of cocoon bucket, water is about 1.5 times of silkworm cocoon volume, warm water in adjusting process by layer out Temperature setting be 60 DEG C, handling duration is set as 1-2 minutes;
Silk cocoon after cocoon cooking: being put into 80 DEG C of soda bath by c) degreasing, and caustic soda and water ratio are 1.5 ratios in degreasing process 100, and impregnate 50-60 minutes;
D) it dials cocoon: the silk cocoon after degreasing being carried out to dial cocoon by hand, silk cocoon is dialled one by one on hand, silkworm chrysalis and Qi Hei are plucked The husking of color is dialled cocoon process and is carried out in clean circulating water, and large aperture filter screen is arranged and is filtered;
E) it opens and dials: will dial and formed on model on the cotton after cocoon to it on such as arciform bamboo model, uniformly to be spread out to cloth The silk floss pocket (also known as cotton cap) of arc-shaped;
F) clear drift: ready-made silk floss pocket is de- dry using clear water immersion;
G) air dry: the silk floss pocket of Tuo Ganhou is dried, when shine to seventy percent it is dry after go to shady and cool region and carry out air dry;
H) it draws: in such a way that four people draw, " cap " being pulled into whole cup size, by four people while well layer by layer of having an effect Word laying fixes core paths crisscross footpaths between fields layer by layer using " full width plane net changes " technique;
I) core detects: being sampled detection to every group of core, and formulates " examining report ", to effective component, heavyweight Weaving method etc. is labeled.
Embodiment 2:
The present invention provides a kind of manufacture crafts of gold silk foster skin quilt, and described specific step is as follows:
A) it selects silkworm: selecting without obvious damaged or slight crack spun gold silkworm silk cocoon;
B) cocoon cooking:
1. dipping: cocoon being immersed in warm water, cocoon layer is made to seep profit, and makes to tie water membrane outside cocoon layer, to enhance water flowing Can, improve it is anti-boils ability, warm water temperature is set as 50-70 DEG C in impregnation technology, and when immersion is about 2-4 minutes a length of;
2. infiltration: using temperature difference permeating method, silk cocoon is first put into steaming part for permeation, osmosizing portion temperature is set in osmosis process 100 DEG C are set to, steam pressure is 0.05 kg/m2, steam and cocoon chamber air are replaced, cocoon is then moved to about 60 DEG C water at low temperature in, because temperature declines, the intracavitary steam of cocoon and air to the cold after sharply shrink, keep the intracavitary external pressure of cocoon different, Achieve the purpose that cocoon layer seeps profit;
3. boiling: carrying out boiling to the cocoon for having seeped profit, main function is to make cocoon chamber guttation and cooked cocoon layer, i.e. raising cocoon layer The temperature of middle water, enters hydrone inside silk gum, increases silk gum volume, softens its swelling, while utilizing hot soup dissolution one Part silk gum, digesting technoloy environment are set as under conditions of steam pressure 0.8-1.0KG/cm2,100 DEG C of temperature;
4. adjustment: the cocoon of boiling first handled in warm water before cocoon out, and solidified outer layer silk gum slightly, to protect cocoon Cocoon, should be placed in after cocoon in about 50 DEG C of water temperature of cocoon bucket, water is about 1.5 times of silkworm cocoon volume, warm water in adjusting process by layer out Temperature setting be 60 DEG C, handling duration is set as 1-2 minutes;
Silk cocoon after cocoon cooking: being put into 80 DEG C of soda bath by c) degreasing, and caustic soda and water ratio are 1.5 ratios in degreasing process 100, and impregnate 50-60 minutes;
D) it dials cocoon: the silk cocoon after degreasing being carried out to dial cocoon by hand, silk cocoon is dialled one by one on hand, silkworm chrysalis and Qi Hei are plucked The husking of color is dialled cocoon process and is carried out in clean circulating water, and large aperture filter screen is arranged and is filtered;
E) it opens and dials: will dial and formed on model on the cotton after cocoon to it on such as arciform bamboo model, uniformly to be spread out to cloth The silk floss pocket (also known as cotton cap) of arc-shaped;
F) clear drift: ready-made silk floss pocket is de- dry using clear water immersion;
G) air dry: the silk floss pocket of Tuo Ganhou is dried, when shine to seventy percent it is dry after go to shady and cool region and carry out air dry;
H) it draws: in such a way that four people draw, " cap " being pulled into whole cup size, by four people while well layer by layer of having an effect Word laying fixes core paths crisscross footpaths between fields layer by layer using " full width plane net changes " technique;
I) core detects: being sampled detection to every group of core, and formulates " examining report ", to effective component, heavyweight Weaving method etc. is labeled.
Embodiment 3:
The present invention provides a kind of manufacture crafts of gold silk foster skin quilt, and described specific step is as follows:
A) it selects silkworm: selecting without obvious damaged or slight crack spun gold silkworm silk cocoon;
B) cocoon cooking:
1. dipping: cocoon being immersed in warm water, cocoon layer is made to seep profit, and makes to tie water membrane outside cocoon layer, to enhance water flowing Can, improve it is anti-boils ability, warm water temperature is set as 50-70 DEG C in impregnation technology, and when immersion is about 2-4 minutes a length of;
2. infiltration: using temperature difference permeating method, silk cocoon is first put into steaming part for permeation, osmosizing portion temperature is set in osmosis process 100 DEG C are set to, steam pressure is 0.05 kg/m2, steam and cocoon chamber air are replaced, cocoon is then moved to about 60 DEG C water at low temperature in, because temperature declines, the intracavitary steam of cocoon and air to the cold after sharply shrink, keep the intracavitary external pressure of cocoon different, Achieve the purpose that cocoon layer seeps profit;
3. boiling: carrying out boiling to the cocoon for having seeped profit, main function is to make cocoon chamber guttation and cooked cocoon layer, i.e. raising cocoon layer The temperature of middle water, enters hydrone inside silk gum, increases silk gum volume, softens its swelling, while utilizing hot soup dissolution one Part silk gum, digesting technoloy environment are set as under conditions of steam pressure 0.8-1.0KG/cm2,100 DEG C of temperature;
4. adjustment: the cocoon of boiling first handled in warm water before cocoon out, and solidified outer layer silk gum slightly, to protect cocoon Cocoon, should be placed in after cocoon in about 50 DEG C of water temperature of cocoon bucket, water is about 1.5 times of silkworm cocoon volume, warm water in adjusting process by layer out Temperature setting be 60 DEG C, handling duration is set as 1-2 minutes;
Silk cocoon after cocoon cooking: being put into 80 DEG C of soda bath by c) degreasing, and caustic soda and water ratio are 1.5 ratios in degreasing process 100, and impregnate 50-60 minutes;
D) it dials cocoon: the silk cocoon after degreasing being carried out to dial cocoon by hand, silk cocoon is dialled one by one on hand, silkworm chrysalis and Qi Hei are plucked The husking of color is dialled cocoon process and is carried out in clean circulating water, and large aperture filter screen is arranged and is filtered;
E) it opens and dials: will dial and formed on model on the cotton after cocoon to it on such as arciform bamboo model, uniformly to be spread out to cloth The silk floss pocket (also known as cotton cap) of arc-shaped;
F) clear drift: ready-made silk floss pocket is de- dry using clear water immersion;
G) air dry: the silk floss pocket of Tuo Ganhou is dried, when shine to seventy percent it is dry after go to shady and cool region and carry out air dry;
H) it draws: by the way of double drawing, will be fixed after silk screen is bonded from level to level;
I) core detects: being sampled detection to every group of core, and formulates " examining report ", to effective component, heavyweight Weaving method etc. is labeled.
Embodiment 4:
It takes gold silk core sample obtained by above-described embodiment 1-3 to be detected respectively, divides three groups to try out three respectively The gold silk core prepared in a embodiment, obtains following data:
As seen from the above table, manufacture craft is preferable in embodiment 2, and after user's use, the sense of touch silk of gold silk foster skin quilt is sliding And complete appearance, it is not susceptible to the case where core misplaces after long-time use, guarantees its service life.
Last: the foregoing is only a preferred embodiment of the present invention, is not intended to restrict the invention, all in the present invention Spirit and principle within, any modification, equivalent replacement, improvement and so on, should be included in protection scope of the present invention it It is interior.

Claims (7)

1. a kind of manufacture craft of gold silk foster skin quilt, it is characterised in that: described specific step is as follows:
A) it selects silkworm: selecting without obvious damaged or slight crack spun gold silkworm silk cocoon;
B) cocoon cooking:
1. dipping: cocoon being immersed in warm water, cocoon layer is made to seep profit, and mentions knot water membrane outside cocoon layer to enhance water flowing performance Highly resistance boils ability;
2. infiltration: using temperature difference permeating method, silk cocoon is first put into steaming part for permeation, sets steam and cocoon chamber air Change, then cocoon moved in about 60 DEG C of water at low temperature, because temperature declines, the intracavitary steam of cocoon and air to the cold after sharply shrink, Keep the intracavitary external pressure of cocoon different, achievees the purpose that cocoon layer seeps profit;
3. boiling: carrying out boiling to the cocoon for having seeped profit, main function is to make cocoon chamber guttation and cooked cocoon layer, i.e. water in raising cocoon layer Temperature, enter hydrone inside silk gum, increase silk gum volume, make its swelling soften, while using hot soup dissolve a part Silk gum;
4. adjustment: the cocoon of boiling first handled in warm water before cocoon out, and solidified outer layer silk gum slightly, to protect cocoon layer, out Cocoon should be placed in after cocoon in about 50 DEG C of water temperature of cocoon bucket, water is about 1.5 times of silkworm cocoon volume;
C) silk cocoon after cocoon cooking degreasing: is put into 80 DEG C of soda bath;
D) it dials cocoon: the silk cocoon after degreasing being carried out to dial cocoon by hand, silk cocoon is dialled one by one and on hand, is plucking silkworm chrysalis and its black Husking;
E) it opens and dials: will dial and form arch on model to it on such as arciform bamboo model, uniformly to be spread out to cloth on the cotton after cocoon The silk floss pocket (also known as cotton cap) of shape;
F) clear drift: ready-made silk floss pocket is de- dry using clear water immersion;
G) air dry: the silk floss pocket of Tuo Ganhou is dried, when shine to seventy percent it is dry after go to shady and cool region and carry out air dry;
H) it draws: in such a way that four people draw, " cap " being pulled into whole cup size, by four people while the Jing Zipu layer by layer that has an effect It is folded, using " full width plane net changes " technique, fix core paths crisscross footpaths between fields layer by layer;
I) core detects: being sampled detection to every group of core, and formulates " examining report ", weaves to effective component, heavyweight Method etc. is labeled.
2. a kind of manufacture craft of gold silk foster skin quilt according to claim 1, it is characterised in that: the impregnation technology Middle warm water temperature is set as 50-70 DEG C, and when immersion is about 2-4 minutes a length of.
3. a kind of manufacture craft of gold silk foster skin quilt according to claim 1, it is characterised in that: the digesting technoloy Environment is set as under conditions of steam pressure 0.8-1.0KG/cm2,100 DEG C of temperature.
4. a kind of manufacture craft of gold silk foster skin quilt according to claim 1, it is characterised in that: the adjusting process The temperature setting of middle warm water is 60 DEG C, and handling duration is set as 1-2 minutes.
5. a kind of manufacture craft of gold silk foster skin quilt according to claim 1, it is characterised in that: described group of cocoon process It is carried out in clean circulating water, and large aperture filter screen is set and is filtered.
6. a kind of manufacture craft of gold silk foster skin quilt according to claim 1, it is characterised in that: the osmosis process Middle osmosizing portion temperature setting is 100 DEG C, and steam pressure is 0.05 kg/m2
7. a kind of manufacture craft of gold silk foster skin quilt according to claim 1, it is characterised in that: the degreasing process Middle caustic soda and water ratio are 1.5 to 100, and are impregnated 50-60 minutes.
CN201910693798.5A 2019-07-30 2019-07-30 A kind of manufacture craft of gold silk foster skin quilt Pending CN110257924A (en)