CN112242589A - Polymer and ceramic composite coating diaphragm, preparation method thereof and lithium ion battery - Google Patents

Polymer and ceramic composite coating diaphragm, preparation method thereof and lithium ion battery Download PDF

Info

Publication number
CN112242589A
CN112242589A CN202011120959.0A CN202011120959A CN112242589A CN 112242589 A CN112242589 A CN 112242589A CN 202011120959 A CN202011120959 A CN 202011120959A CN 112242589 A CN112242589 A CN 112242589A
Authority
CN
China
Prior art keywords
coating
ceramic
polymer
base film
diaphragm
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN202011120959.0A
Other languages
Chinese (zh)
Inventor
刘向春
唐丽
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shenzhen Dingtaixiang New Energy Technology Co ltd
Original Assignee
Shenzhen Dingtaixiang New Energy Technology Co ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shenzhen Dingtaixiang New Energy Technology Co ltd filed Critical Shenzhen Dingtaixiang New Energy Technology Co ltd
Priority to CN202011120959.0A priority Critical patent/CN112242589A/en
Publication of CN112242589A publication Critical patent/CN112242589A/en
Pending legal-status Critical Current

Abstract

The application discloses a polymer and ceramic composite coating diaphragm, a preparation method thereof and a lithium ion battery. The preparation method of the polymer and ceramic composite coating diaphragm comprises the steps of preparing a ceramic coating on a base film, filling micropores and holes of the base film with a filling solvent in advance before performing oily coating on the ceramic coating, and then performing oily coating; after the oily coating is finished, immersing the ceramic coating diaphragm subjected to the oily coating into an extraction solvent, and extracting the filling solvent from micropores of the base film and pores of the ceramic coating layer while extracting and hardening the coating layer; and finally, drying to obtain the polymer and ceramic composite coating diaphragm. This application is when carrying out oily coating, and polymer powder is difficult for getting into in base film micropore and the ceramic coating hole to solved oily coating and blockked up the problem in base film micropore and ceramic coating hole easily, and kept the good advantage of oily coating cohesiveness.

Description

Polymer and ceramic composite coating diaphragm, preparation method thereof and lithium ion battery
Technical Field
The application relates to the field of lithium ion battery diaphragm materials, in particular to a polymer and ceramic composite coating diaphragm, a preparation method thereof and a lithium ion battery.
Background
Lithium ion batteries are widely used because of their many advantages, such as high energy density, no memory effect, long cycle life, etc. Generally, a lithium ion battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, a separator, and a battery case. Among them, the separator is referred to as the "third pole" of the battery because of its critical role in lithium ion batteries.
The separator is a separator between the positive and negative electrodes of the battery, and is required to have good electrical insulation and air permeability. In current lithium ion batteries, polyolefin is generally used as a separator (or base film). In order to improve thermal stability, oxidation resistance, thermal shrinkage resistance, absorption of liquid electrolyte, wettability, and liquid-absorbing and liquid-retaining ability of the separator, etc., it is generally necessary to perform ceramic coating and polymer coating on the surface of the polyolefin separator to form a ceramic coating and a polymer coating on the base film. Among them, the production processes of the polymer-coated separator are mainly classified into two major types, water-based coating and oil-based coating. The aqueous coating is to adopt water as a solvent to prepare polymer coating slurry for coating, and has the advantages of low production cost, small environmental pollution and the like; however, the polymer coating formed by aqueous coating has weak adhesion with positive and negative electrode sheets, and is prone to generate phenomena such as poor hot pressing with the electrode sheets. The oily coating is to adopt organic solvent to prepare polymer coating slurry for coating, and the oily coating adopts organic solvent, so that the polymer coating has better adhesion with the positive and negative pole pieces, and the defect of weak adhesion of the aqueous coating polymer coating are overcome; however, the oily coating tends to block the pores of the base film and the ceramic coating, resulting in a phenomenon of poor air permeability.
In addition to aqueous coating and oily coating, studies have been made to use an oil-water mixed system, that is, a mixed solvent of an organic solvent and water is used to prepare a polymer coating slurry; although the method relieves the problems that the water-based coating has weak cohesiveness and the oil-based coating is easy to block micropores to a certain extent; however, this is only a balance of adhesion and cost; in general, mixed solvent coatings are less cohesive than oil coatings, are more costly than water-based coatings, and are environmentally unfriendly.
Therefore, how to solve the problem that the oil coating easily blocks micropores of the base film and holes of the ceramic coating on the basis of ensuring the cohesiveness of the oil coating is the key point and difficulty of the research of the polymer and ceramic composite coating diaphragm.
Disclosure of Invention
The application aims to provide a preparation method of a polymer and ceramic composite coating diaphragm, the polymer and ceramic composite coating diaphragm prepared by the preparation method, and a lithium ion battery adopting the polymer and ceramic composite coating diaphragm.
In order to achieve the purpose, the following technical scheme is adopted in the application:
the first aspect of the application discloses a preparation method of a polymer and ceramic composite coating diaphragm, which comprises the steps of preparing a ceramic coating on a base film, preparing the polymer coating on the ceramic coating diaphragm by adopting oil coating after the ceramic coating diaphragm is obtained, filling micropores of the base film and holes of the ceramic coating by adopting a filling solvent in advance before the oil coating is carried out, and then carrying out the oil coating; after the oily coating is finished, immersing the ceramic coating diaphragm subjected to the oily coating into an extraction solvent, and extracting the filling solvent from micropores of the base film and the hole groups of the ceramic coating while carrying out extraction hardening on the coating; and finally, drying to obtain the polymer and ceramic composite coating diaphragm.
The preparation method has the advantages that after the ceramic coating is prepared on the base film, the micropores of the base film and the holes of the ceramic coating are filled in advance, so that polymer powder is not easy to enter the micropores of the base film and the holes of the ceramic coating when oil coating is carried out, and the problem that the micropores of the base film and the holes of the ceramic coating are easy to block due to the oil coating is solved; in addition, the preparation method better retains the advantage of good cohesiveness of the oily coating.
In one implementation of the present application, the filling solvent is at least one of ethanol, acetone, glycerol, propylene glycol, isopropanol, butanol, isobutanol, ethylene glycol, and diethylene glycol.
It should be noted that the filling solvent used in the present application needs to pay attention to two aspects, firstly, the filling solvent can be filled into the micropores of the base film and the pores of the ceramic coating to prevent the polymer powder from entering; secondly, can conveniently follow-up adopting the extraction solvent to extract it from base film micropore and ceramic coating hole, perhaps, can conveniently release from the micropore in follow-up processing, for example can follow-up evaporation when drying out. It is to be understood that any solvent or mixed solution satisfying the above two points can be used in the present application.
In one implementation of the present application, the extraction solvent is water or a mixed solvent of water and an organic solvent. Wherein the weight ratio of the organic solvent in the mixed solvent is not more than 60 wt%. Wherein, a mixed solvent containing an organic solvent is adopted, and the effect is to utilize the content of the organic solvent to regulate and control the extraction speed of the polymer slurry and the pore-forming effect of the coating; generally, the lower the organic solvent content, the faster the extraction rate, and the larger the pores of the polymer slurry forming the coating.
In one implementation of the present application, the organic solvent in the mixed solvent is the same as the organic solvent used for the oily coating.
In one implementation of the present application, the organic solvent is at least one of dimethylacetamide, acetone, N-methylpyrrolidone, and dimethylsulfoxide.
The extraction solvent of the present application is used to harden the coating layer and to extract the filling solvent from the pores of the base film. Therefore, when the filling solvent is a solvent having a good water solubility, such as ethanol, acetone, glycerol, propylene glycol, isopropanol, butanol, isobutanol, ethylene glycol, and diethylene glycol, water can be directly used as the extraction solvent.
In one implementation of the present application, the base film is at least one of a dry-stretched microporous film, a wet-stretched microporous film, and a non-woven microporous film.
The base film, i.e. the conventional single-layer or multi-layer composite diaphragm, can be a dry-stretched microporous film, a wet-stretched microporous film or a non-woven microporous film; as for the material of the base film, polyolefin such as polyethylene, polypropylene, etc. can be mentioned.
In one implementation of the present application, the base film is a polyolefin microporous film.
In one implementation of the present application, the polyolefin microporous membrane is a polyethylene microporous membrane, a polypropylene microporous membrane, or a composite membrane of a polyethylene microporous membrane and a polypropylene microporous membrane.
In one implementation of the present application, the solid content of the polymer slurry used for oil coating is 5% to 40%. Preferably, the polymer syrup has a solids content of 10% to 35%.
In one implementation manner of the application, the polymer slurry comprises 65-95 parts of polymer powder and 1-20 parts of first binder by weight of dry matter; preferably, the polymer powder is 70 to 90 parts.
In one implementation of the present application, the first binder is selected from at least one of poly (meth) acrylic acid, poly (meth) acrylate, butadiene-styrene copolymer, styrene-acrylate copolymer, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyacrylonitrile, polyurethane, (meth) acrylic acid- (meth) acrylate copolymer.
In one implementation of the present application, the polymer powder is at least one of a vinylidene fluoride homopolymer, a vinylidene fluoride copolymer, a methyl methacrylate homopolymer, a methyl methacrylate copolymer, aramid, polyacrylonitrile, and polyethylene oxide.
In one embodiment of the present invention, the polymer powder has a particle size of 0.2 to 10 μm.
In one implementation manner of the present application, the ceramic slurry used for the ceramic coating layer comprises the following components in the amount ratio: 70-95 parts of ceramic particles; 2-20 parts of a second binder; 1-15 parts of a thickening agent; 0.1-3 parts of a dispersing agent;
in one implementation of the present application, the ceramic particles are 75-90 parts.
In one implementation of the present application, the second binder is selected from at least one of poly (meth) acrylic acid, poly (meth) acrylate, butadiene-styrene copolymer, styrene-acrylate copolymer, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyacrylonitrile, polyurethane, and (meth) acrylic acid- (meth) acrylate copolymer.
In one implementation of the present application, the thickener is at least one of carboxymethyl cellulose, carboxyethyl cellulose, polyvinyl alcohol, sodium alginate, polyethylene oxide, polyurethane, polyacrylamide, and guar gum.
In one implementation of the present application, the dispersant is at least one of polyacrylate, polyglycol ether, and phosphate compound.
A second aspect of the present application discloses a polymer and ceramic composite coated separator prepared by the preparation method of the present application.
Compared with the polymer and ceramic composite coating membrane prepared by conventional oily coating, the polymer and ceramic composite coating membrane prepared by the method has the advantages that the ventilation value of the coated polymer and ceramic composite coating membrane is only 9-26s/cc relative to that of the ceramic coating membrane, the permeability is better, and the use requirement of the battery membrane can be better met; in addition, the preparation method is essentially oil-based coating, so that the polymer coating and the ceramic coating have good cohesiveness, and the powder falling phenomenon is avoided.
A third aspect of the present application discloses a lithium ion battery employing the polymer and ceramic composite coated separator of the present application.
The lithium ion battery has the advantages that due to the fact that the polymer and ceramic composite coating diaphragm is adopted, firstly, the diaphragm is good in air permeability, the polymer coating is good in cohesiveness and not prone to falling, and the powder falling phenomenon is avoided; secondly, the polymer coating of the polymer and ceramic composite coating diaphragm and the pole piece have good hot-pressing stability, and the comprehensive properties of the lithium ion battery such as stability and safety are improved.
Due to the adoption of the technical scheme, the beneficial effects of the application are as follows:
according to the preparation method of the polymer and ceramic composite coating diaphragm, after the ceramic coating is prepared on the base film and before the oily coating, the micropores of the base film and the holes of the ceramic coating are protected by the filling solvent creatively in advance, so that the micropores of the base film and the holes of the ceramic coating are not easy to block during the oily coating, and finally the filling solvent is extracted from the micropores and the holes, so that the problem that the micropores of the base film are easy to block during the oily coating is solved on the basis of ensuring the cohesiveness of the oily coating.
Detailed Description
The present application will be described in further detail with reference to specific embodiments. In the following description, numerous details are set forth in order to provide a better understanding of the present application. However, those skilled in the art will readily recognize that some of the features may be omitted or replaced with other elements, materials, methods in different instances. In some instances, certain operations related to the present application have not been shown or described in detail in order to avoid obscuring the core of the present application from excessive description, and it is not necessary for those skilled in the art to describe these operations in detail, so that they may be fully understood from the description in the specification and the general knowledge in the art.
Furthermore, the features, operations, or characteristics described in the specification may be combined in any suitable manner to form various embodiments. Also, the various steps or actions in the method descriptions may be transposed or transposed in order, as will be apparent to one of ordinary skill in the art. Thus, the various sequences in the specification are for the purpose of clearly describing one embodiment only and are not meant to be necessarily order unless otherwise indicated where a certain order must be followed.
Reagent and apparatus
Unless otherwise indicated, the materials and reagents used in the examples of the present application are commercially available products that are conventionally used in the production of lithium battery-related materials.
In the examples of the present application, the stirring was performed using a 149L double planetary power mixer manufactured by Guangzhou Hongshang machinery manufacturing Co.
In the embodiment of the application, after the ceramic coating is prepared on the base film, solvent is creatively filled in the micropores of the base film and the holes of the ceramic coating in advance for protection before oily coating, so that the micropores of the base film and the holes of the ceramic coating are not easily blocked during oily coating, and the problem that the micropores of the base film and the holes of the ceramic coating are easily blocked by oily coating is solved on the basis of ensuring the cohesiveness of the oily coating; furthermore, the polymer and ceramic composite coating diaphragm prepared by the embodiment has better air permeability, the polymer coating and the pole piece of the polymer and ceramic composite coating diaphragm have good hot-pressing stability, and the comprehensive properties of the lithium ion battery, such as stability, safety and the like, are improved.
In the examples of the present application, a ceramic coating slurry was prepared by taking alumina as an example, and was coated on a polyethylene-based film to prepare a ceramic-coated separator, which was used in each example and comparative example to further prepare a polymer and ceramic composite-coated separator. Among them, the polyethylene-based film is a 5 μm separator commercially available from Asahi Kasei chemical electronic Material Co.
The specific preparation method of the ceramic coating diaphragm in the embodiment of the application is as follows:
1. mixing 80 parts of alumina, 15 parts of poly (meth) acrylic acid with a solid content of 50% and 120 parts of deionized water, stirring at 30 ℃ and 1200rpm for 1h, then adding 100 parts of a thickening agent (2% CMC premixed aqueous solution) and 0.5 part of polyethylene glycol ether, and stirring at 30 ℃ and 1000rpm for 1.5h to obtain ceramic slurry;
2. and coating the ceramic slurry on one side of a 5-micron polyethylene film through micro-gravure coating, and drying to obtain the ceramic coated diaphragm with the thickness of a ceramic layer of 2 microns.
Example 1
In the method, acetone is used as a filling solvent, before the ceramic coating diaphragm is subjected to oily coating, the micropores of the base film and the holes of the ceramic coating are filled with the acetone in advance, after the oily coating is finished, water is used as an extraction solvent to perform soaking extraction on the coated ceramic coating diaphragm, and finally, the polymer and ceramic composite coating diaphragm is obtained by drying.
The specific preparation method of the polymer and ceramic composite coating diaphragm of the embodiment is as follows:
preparation of polymer coating slurry: 70 parts of polyvinylidene fluoride-hexafluoroethylene (PVDF-HFP), 8 parts of polymethacrylic acid, 702 parts of dimethylacetamide were mixed and stirred at 30 ℃ and 1500rpm for 1 hour to obtain a polymer slurry having a solid content of about 10 wt%.
Preparation of polymer and ceramic composite coated separator: before the ceramic coating diaphragm is subjected to oil coating, acetone is adopted to fill micropores of a base film and holes of a ceramic coating layer of the ceramic coating diaphragm in advance, then oil coating is carried out, and the polymer coating slurry prepared in the embodiment is coated on one side of the filled ceramic coating diaphragm through a micro-gravure; after the oily coating is finished, soaking the coated ceramic coating diaphragm into a water solvent, and extracting an acetone solvent from micropores of the base film and holes of the ceramic coating while extracting and hardening the coating; finally, the polymer and ceramic composite coating membrane of the example is obtained after three-stage baking and drying treatment at 45 ℃, 55 ℃ and 45 ℃, wherein the thickness of the PVDF-HFP coating layer is about 2 mu m.
Example 2
In the method, glycerin is used as a filling solvent, micropores of a base film and pores of a ceramic coating are filled before the ceramic coating diaphragm is subjected to oily coating, 10 wt% of N-methyl pyrrolidone containing 10 wt% of N-methyl pyrrolidone is used as an extraction solvent for soaking and extraction after the oily coating is performed, and finally, the polymer and ceramic composite coating diaphragm is obtained after drying.
The specific preparation method of the polymer and ceramic composite coating diaphragm of the embodiment is as follows:
preparation of polymer coating slurry: 90 parts of PVDF-HFP, 20 parts of polymethacrylic acid and 165 parts of N-methylpyrrolidone were mixed and stirred at 30 ℃ and 1500rpm for 1 hour to obtain a polymer coating syrup having a solid content of about 40% by weight.
Preparation of polymer and ceramic composite coated separator: before the ceramic coating diaphragm is subjected to oily coating, the micropores of the base film and the holes of the ceramic coating layer of the ceramic coating diaphragm are filled with glycerol in advance, then the oily coating is carried out, and the polymer coating slurry prepared in the embodiment is coated on one side of the filled ceramic coating diaphragm through a micro-gravure; after the oily coating is finished, the coated ceramic coating diaphragm is immersed into water containing 10 wt% of N-methyl pyrrolidone, and glycerin is extracted from micropores of the base film and holes of the ceramic coating while the coating is extracted and hardened; finally, the polymer and ceramic composite coating membrane of the example is obtained after three-stage baking and drying treatment at 45 ℃, 55 ℃ and 45 ℃, wherein the thickness of the PVDF-HFP coating layer is about 4 mu m.
Example 3
In the method, ethanol is used as a filling solvent, micropores of a base film and pores of a ceramic coating are filled before the ceramic coating diaphragm is subjected to oily coating, water containing 30 wt% of acetone is used as an extraction solvent for soaking and extraction after the oily coating is performed, and finally the polymer and ceramic composite coating diaphragm is obtained by drying.
The specific preparation method of the polymer and ceramic composite coating diaphragm of the embodiment is as follows:
preparation of polymer coating slurry: 70 parts of PVDF-HFP, 8 parts of polymethacrylic acid and 702 parts of acetone were mixed and stirred at 30 ℃ and 1500rpm for 1 hour to obtain a polymer coating syrup having a solid content of about 10% by weight.
Preparation of polymer and ceramic composite coated separator: before the ceramic coating diaphragm is subjected to oily coating, ethanol is adopted to fill micropores of a base film and holes of a ceramic coating of the ceramic coating diaphragm in advance, then the oily coating is carried out, and the polymer coating slurry prepared in the embodiment is coated on two sides of the filled ceramic coating diaphragm through a micro-gravure; after the oily coating is finished, the coated ceramic coating diaphragm is immersed into water containing 30 wt% of acetone, and ethanol is extracted from micropores of the base film and holes of the ceramic coating while the coating is extracted and hardened; finally, after three-stage baking and drying treatment at 45 ℃, 55 ℃ and 45 ℃, the polymer and ceramic composite coating diaphragm of the embodiment is obtained, wherein the thickness of the PVDF-HFP coating on each side is about 2 μm.
Example 4
In the embodiment, acetone is used as a filling solvent to fill micropores of a base film and holes of a ceramic coating, after oily coating, 60 wt% of dimethylacetamide is used as an extraction solvent to perform soaking extraction, and finally drying is performed to obtain the polymer and ceramic composite coating diaphragm.
The specific preparation method of the polymer and ceramic composite coating diaphragm of the embodiment is as follows:
preparation of polymer coating slurry: 70 parts of methyl methacrylate homopolymer, 8 parts of polymethacrylic acid and 702 parts of dimethylacetamide were mixed and stirred at 30 ℃ and 1500rpm for 1 hour to obtain a polymer coating syrup having a solid content of about 10 wt%.
Preparation of polymer and ceramic composite coated separator: before the ceramic coating diaphragm is subjected to oil coating, acetone is adopted to fill micropores of a base film and holes of a ceramic coating layer of the ceramic coating diaphragm in advance, then oil coating is carried out, and the polymer coating slurry prepared in the embodiment is coated on one side of the filled ceramic coating diaphragm through a micro-gravure; after the oily coating is finished, the coated ceramic coating diaphragm is immersed into dimethylacetamide containing 60 wt%, and acetone is extracted from micropores of the base film and holes of the ceramic coating while the coating is extracted and hardened; finally, the polymer and ceramic composite coating diaphragm of the embodiment is obtained after three-stage baking and drying treatment at 45 ℃, 55 ℃ and 45 ℃, wherein the thickness of the methyl methacrylate homopolymer coating is about 2 mu m.
Example 5
In the embodiment, butanol is used as a filling solvent to fill micropores of the base film and holes of the ceramic coating, water is used as an extraction solvent to perform soaking extraction after oily coating is performed, and finally, the polymer and ceramic composite coating diaphragm is obtained after drying.
The specific preparation method of the polymer and ceramic composite coating diaphragm of the embodiment is as follows:
preparation of polymer coating slurry: 90 parts of methyl methacrylate homopolymer, 20 parts of polymethacrylic acid and 165 parts of dimethyl sulfoxide were mixed and stirred at 30 ℃ and 1500rpm for 1 hour to obtain a polymer coating slurry having a solid content of about 40 wt%.
Preparation of polymer and ceramic composite coated separator: before the ceramic coating diaphragm is subjected to oily coating, the micropores of the base film and the pores of the ceramic coating layer of the ceramic coating diaphragm are filled with butanol in advance, then the oily coating is carried out, and the polymer coating slurry prepared in the embodiment is coated on one side of the filled ceramic coating diaphragm through a micro-gravure; after the oily coating is finished, the coated ceramic coating diaphragm is immersed in water, and butanol is extracted from micropores of the base film and holes of the ceramic coating while the coating is extracted and hardened; finally, the polymer and ceramic composite coating diaphragm of the embodiment is obtained after three-stage baking and drying treatment at 45 ℃, 55 ℃ and 45 ℃, wherein the thickness of the methyl methacrylate homopolymer coating is about 4 mu m.
Example 6
The preparation method adopts ethylene glycol as a filling solvent to fill micropores of a base film and holes of a ceramic coating, adopts water as an extraction solvent to perform soaking extraction after oil coating, and finally obtains the polymer and ceramic composite coating diaphragm of the preparation method through drying.
The specific preparation method of the polymer and ceramic composite coating diaphragm of the embodiment is as follows:
preparation of polymer coating slurry: 70 parts of methyl methacrylate homopolymer, 8 parts of polymethacrylic acid and 702 parts of dimethylacetamide were mixed and stirred at 30 ℃ and 1500rpm for 1 hour to obtain a polymer coating syrup having a solid content of about 10 wt%.
Preparation of polymer and ceramic composite coated separator: before the ceramic coating diaphragm is subjected to oily coating, the micropores of the base film and the holes of the ceramic coating layer of the ceramic coating diaphragm are filled with glycol in advance, then the oily coating is carried out, and the polymer coating slurry prepared in the embodiment is coated on the two sides of the filled ceramic coating diaphragm through a micro-gravure; after the oily coating is finished, the coated ceramic coating diaphragm is immersed in water, and glycol is extracted from micropores of the base film and holes of the ceramic coating while the coating is extracted and hardened; finally, the polymer and ceramic composite coating membrane of the example is obtained after three-stage baking and drying treatment at 45 ℃, 55 ℃ and 45 ℃, wherein the thickness of the methyl methacrylate homopolymer coating on each side is about 2 mu m.
Comparative example 1
In the embodiment, as a comparative example, the micropores of the base film and the pores of the ceramic coating are not filled with a filling solvent, the ceramic coating diaphragm is coated with oil, then soaked and extracted by using water as an extraction solvent, and finally dried to obtain the polymer and ceramic composite coating diaphragm.
The specific preparation method of the polymer and ceramic composite coating diaphragm of the embodiment is as follows:
preparation of polymer coating slurry: 70 parts of PVDF-HFP, 8 parts of polymethacrylic acid and 702 parts of dimethylacetamide were mixed and stirred at 30 ℃ and 1500rpm for 1 hour to obtain a polymer coating syrup having a solid content of about 10% by weight.
Preparation of polymer and ceramic composite coated separator: performing oil coating on the ceramic-coated separator, and coating the polymer coating slurry prepared in the present comparative example on one side of the ceramic-coated separator by means of a micro-gravure; after the oily coating is finished, the coated ceramic coating diaphragm is immersed in water, and the coating is subjected to extraction hardening; finally, the polymer and ceramic composite coating diaphragm of the embodiment is obtained after three-stage baking and drying treatment at 45 ℃, 55 ℃ and 45 ℃, wherein the thickness of the methyl methacrylate homopolymer coating is about 2 mu m.
Comparative example 2
In this example, as a comparative example, pores of the base film and pores of the ceramic coating layer were filled without using a filling solvent, and after oil-coating was performed on the ceramic-coated separator, water containing 10 wt% of N-methylpyrrolidone was used as an extraction solvent to perform immersion extraction, and finally dried to obtain the polymer and ceramic composite-coated separator of this example.
The specific preparation method of the polymer and ceramic composite coating diaphragm of the embodiment is as follows:
preparation of polymer coating slurry: 90 parts of PVDF-HFP, 20 parts of polymethacrylic acid and 165 parts of N-methylpyrrolidone were mixed and stirred at 30 ℃ and 1500rpm for 1 hour to obtain a polymer coating syrup having a solid content of about 40% by weight.
Preparation of polymer and ceramic composite coated separator: performing oil coating on the ceramic-coated separator, and coating the polymer coating slurry prepared in the present comparative example on one side of the ceramic-coated separator by means of a micro-gravure; after the oil coating is finished, the coated ceramic coating diaphragm is immersed into water containing 10 wt% of N-methyl pyrrolidone, and the coating is subjected to extraction hardening; finally, the polymer and ceramic composite coating diaphragm of the embodiment is obtained after three-stage baking and drying treatment at 45 ℃, 55 ℃ and 45 ℃, wherein the thickness of the methyl methacrylate homopolymer coating is about 4 mu m.
Comparative example 3
In this example, as a comparative example, micropores of the base film and pores of the ceramic coating layer were filled without using a filling solvent, and after oil coating was performed on the ceramic coated membrane, immersion extraction was performed using water containing 60 wt% of acetone as an extraction solvent, and finally drying was performed to obtain the polymer and ceramic composite coated membrane of this example.
The specific preparation method of the polymer and ceramic composite coating diaphragm of the embodiment is as follows:
preparation of polymer coating slurry: 70 parts of PVDF-HFP, 8 parts of polymethacrylic acid and 702 parts of acetone were mixed and stirred at 30 ℃ and 1500rpm for 1 hour to obtain a polymer coating syrup having a solid content of about 10% by weight.
Preparation of polymer and ceramic composite coated separator: performing oil coating on the ceramic-coated separator, and coating the polymer coating slurry prepared in the comparative example on both sides of the ceramic-coated separator by using a micro-gravure; after the oil coating is finished, soaking the coated ceramic coating diaphragm in water containing 30 wt% of acetone, and carrying out extraction hardening on the coating; finally, the polymer and ceramic composite coating membrane of the example is obtained after three-stage baking and drying treatment at 45 ℃, 55 ℃ and 45 ℃, wherein the thickness of the methyl methacrylate homopolymer coating on each side is about 2 mu m.
Experiment 1 air permeability measurement
The measuring method comprises the following steps: the ceramic coated separators and the polymer and ceramic composite coated separators of examples 1 to 6 and the ceramic coated separators and the polymer and ceramic composite coated separators of comparative examples 1 to 3 were taken, and the air permeability values (unit: sec/100cc) were measured using a digital type Wang-type laboratory ventilation machine and the air permeability increase values were calculated, and the results are shown in Table 1.
TABLE 1 air permeability values (sec/100cc)
Air permeability value of ceramic coated membrane Polymer and ceramic composite coated membranes air permeability values Increase in ventilation value
Example 1 108 117 9
Example 2 110 128 18
Example 3 109 135 26
Example 4 108 127 19
Example 5 109 127 18
Example 6 110 127 17
Comparative example 1 107 133 26
Comparative example 2 109 167 58
Comparative example 3 109 171 62
The air permeability value reflects the permeability of the membrane, and the air permeability value is the smaller the time (seconds) for 100mL of air to penetrate through a membrane with a certain area under a certain pressure in an air permeability instrument. As can be seen from the data in Table 1, the permeability increase of the polymer and ceramic composite coated membranes of comparative examples 1-3 is significantly greater, while the permeability increase of the polymer and ceramic composite coated membranes of examples 1-6 is significantly less, indicating that the permeability of the polymer and ceramic composite coated membranes of examples 1-6 is greatly improved.
Experiment 2 testing of Heat shrinkage of separator
Using an instrument: high-precision industrial oven, film ruler. The polymer and ceramic composite coated membranes of examples 1-6 and the polymer and ceramic composite coated membranes of comparative examples 1-3 were each cut into 100mm x 100mm sample 3 pieces, and the size of the sample was measured after baking in an oven at 105 ℃ for 2 hours, with the length being designated as L1 and the width being designated as L2. The heat shrinkage (MD) in the machine direction was (100mm-L1)/100mm X100%, and the heat shrinkage (TD) in the transverse direction was (100mm-L2)/100mm X100%, taking the arithmetic average of the three samples as the final result. The test results are shown in Table 2.
TABLE 2 Heat shrinkage (%)
Thermal shrinkage Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Comparative example 1 Comparative example 2 Comparative example 3
MD 1.5 1.7 1.7 1.5 1.6 1.7 1.5 1.7 1.8
TD 1.2 1.2 1.2 1.3 1.2 1.2 1.2 1.2 1.4
As can be seen from the data of table 2, the polymer and ceramic composite coated separators of examples 1 to 3 have high heat resistance at the same level as the polymer and ceramic composite coated separators of corresponding comparative examples 1 to 3, that is, the method for preparing the polymer and ceramic composite coated separator of this example can improve the air permeability of the composite separator, and the polymer and ceramic composite coated separator prepared has high heat resistance.
The present application has been described with reference to specific examples, which are provided only to aid understanding of the present application and are not intended to limit the present application. For a person skilled in the art to which the application pertains, several simple deductions, modifications or substitutions may be made according to the idea of the application.

Claims (10)

1. A preparation method of a polymer and ceramic composite coating diaphragm comprises the steps of preparing a ceramic coating on a base film, and preparing the polymer coating by adopting oil coating on the ceramic coating after obtaining the ceramic coating diaphragm, and is characterized by comprising the following steps: before oil coating, filling the micropores of the base film and the holes of the ceramic coating by using a filling solvent in advance, and then performing oil coating; after the oily coating is finished, immersing the ceramic coating diaphragm subjected to the oily coating into an extraction solvent, and extracting the filling solvent from micropores of the base film and holes of the ceramic coating while carrying out extraction hardening on the coating; and finally, drying to obtain the polymer and ceramic composite coating diaphragm.
2. The method of claim 1, wherein: the filling solvent is at least one of ethanol, acetone, glycerol, propylene glycol, isopropanol, butanol, isobutanol, ethylene glycol and diethylene glycol.
3. The method of claim 1, wherein: the extraction solvent is water or a mixed solvent of water and an organic solvent; preferably, the weight ratio of the organic solvent in the mixed solvent is not more than 60 wt%.
4. The production method according to claim 3, characterized in that: the organic solvent in the mixed solvent is the same as the organic solvent adopted for the oily coating;
preferably, the organic solvent is at least one of dimethylacetamide, acetone, N-methylpyrrolidone, and dimethylsulfoxide.
5. The method of claim 1, wherein: the base film is at least one of a dry-method stretched microporous film, a wet-method microporous film and a non-woven fabric microporous film;
preferably, the base film is a polyolefin microporous film;
preferably, the polyolefin microporous membrane is a polyethylene microporous membrane, a polypropylene microporous membrane or a composite membrane of the polyethylene microporous membrane and the polypropylene microporous membrane.
6. The production method according to any one of claims 1 to 5, characterized in that: the solid content of the polymer slurry adopted for the oily coating is 5-40%;
preferably, the solid content of the polymer slurry is 10-35%;
preferably, the polymer slurry comprises 65-95 parts of polymer powder and 1-20 parts of first binder by weight of dry matters;
preferably, the first binder is at least one selected from the group consisting of poly (meth) acrylic acid, poly (meth) acrylate, butadiene-styrene copolymer, styrene-acrylate copolymer, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyacrylonitrile, polyurethane, and (meth) acrylic acid- (meth) acrylate copolymer;
preferably, the polymer powder is 70 to 90 parts.
7. The method of claim 6, wherein: the polymer powder is at least one of vinylidene fluoride homopolymer, vinylidene fluoride copolymer, methyl methacrylate homopolymer, methyl methacrylate copolymer, aramid fiber, polyacrylonitrile and polyethylene oxide;
preferably, the particle size of the polymer powder is 0.2-10 μm.
8. The production method according to any one of claims 1 to 5, characterized in that: the ceramic coating adopts ceramic slurry which comprises the following components in percentage by weight: 70-95 parts of ceramic particles; 2-20 parts of a second binder; 1-15 parts of a thickening agent; 0.1-3 parts of a dispersing agent;
preferably, the second binder is at least one selected from the group consisting of poly (meth) acrylic acid, poly (meth) acrylate, butadiene-styrene copolymer, styrene-acrylate copolymer, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyacrylonitrile, polyurethane, and (meth) acrylic acid- (meth) acrylate copolymer;
preferably, the thickener is at least one of carboxymethyl cellulose, carboxyethyl cellulose, polyvinyl alcohol, sodium alginate, polyethylene oxide, polyurethane, polyacrylamide and guar gum;
preferably, the dispersant is at least one of polyacrylate, polyglycol ether and phosphate compound;
preferably, the ceramic fine particles are 75 to 90 parts.
9. A polymer and ceramic composite coated separator prepared by the preparation method of any one of claims 1 to 8.
10. A lithium ion battery employing the polymer and ceramic composite coated separator of claim 9.
CN202011120959.0A 2020-10-19 2020-10-19 Polymer and ceramic composite coating diaphragm, preparation method thereof and lithium ion battery Pending CN112242589A (en)