CN112898552B - Condensation devolatilization device and method for semi-aromatic polyester-polycarbonate copolymer - Google Patents

Condensation devolatilization device and method for semi-aromatic polyester-polycarbonate copolymer Download PDF

Info

Publication number
CN112898552B
CN112898552B CN202110266157.9A CN202110266157A CN112898552B CN 112898552 B CN112898552 B CN 112898552B CN 202110266157 A CN202110266157 A CN 202110266157A CN 112898552 B CN112898552 B CN 112898552B
Authority
CN
China
Prior art keywords
glue solution
washing
kettle
condensing
devolatilizing
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN202110266157.9A
Other languages
Chinese (zh)
Other versions
CN112898552A (en
Inventor
孟跃中
王文静
梁嘉欣
肖敏
王拴紧
韩东梅
叶淑娴
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sun Yat-sen University
Original Assignee
Sun Yat-sen University
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sun Yat-sen University filed Critical Sun Yat-sen University
Priority to CN202110266157.9A priority Critical patent/CN112898552B/en
Publication of CN112898552A publication Critical patent/CN112898552A/en
Application granted granted Critical
Publication of CN112898552B publication Critical patent/CN112898552B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了半芳香族聚酯‑聚碳酸酯共聚物的凝聚脱挥装置和方法,该方法包括向胶液储罐内加入5~15wt%的水,与胶液储罐内的胶液相混合终止聚合反应;向洗涤凝聚脱挥釜内注入60~90℃的热水,使胶液中的环氧丙烷组分脱出;且调控向洗涤凝聚脱挥釜注入热水的流速与向洗涤凝聚脱挥釜泵入胶液的流速相匹配;由于先采用5~15wt%的水终止聚合反应,再采用60~90℃的热水作为洗涤凝聚剂,高效回收了作为反应物和溶剂的环氧丙烷。可减少聚合后凝聚脱挥时间,明显提高凝聚脱挥效率,显著提高PPC产品的品质,并适用于所有的PPC产品。

The invention discloses a device and method for condensation and devolatilization of semi-aromatic polyester-polycarbonate copolymer. The method includes adding 5 to 15 wt% water into a glue storage tank, and mixing it with the glue in the glue storage tank. Mixing terminates the polymerization reaction; injects hot water of 60 to 90°C into the washing coagulation and devolatilization kettle to remove the propylene oxide component in the glue; and regulates the flow rate of hot water injected into the washing coagulation and devolatilization kettle and the flow rate of the hot water into the washing coagulation and devolatilization kettle. The flow rate of the glue liquid pumped into the devolatilization kettle matches; because 5 to 15 wt% water is first used to terminate the polymerization reaction, and then hot water of 60 to 90°C is used as the washing coagulant, the epoxy as the reactant and solvent is efficiently recovered Propane. It can reduce the coagulation and devolatilization time after polymerization, significantly improve the coagulation and devolatilization efficiency, significantly improve the quality of PPC products, and is applicable to all PPC products.

Description

Apparatus and method for condensing and devolatilizing semi-aromatic polyester-polycarbonate copolymer
Technical Field
The invention relates to a device and a process field for condensing and devolatilizing a polycarbonate copolymer, in particular to a device and a method for condensing and devolatilizing a semi-aromatic polyester-polycarbonate copolymer.
Background
Since the industrial revolution, greenhouse gases with strong heat absorption such as carbon dioxide exhausted into the atmosphere by human beings are increased year by year, and the greenhouse effect of the atmosphere is also enhanced, so that a series of environmental problems are caused, and attention is also brought to countries around the world; as a main gas causing the greenhouse effect, namely carbon dioxide, is one of the most abundant carbon sources on the earth, how to reasonably utilize the carbon dioxide, the greenhouse effect can be effectively reduced, waste is changed into valuable, for example, the polycarbonate can be prepared by using a chemical method to fix, and the carbon dioxide is taken as a raw material to be copolymerized with alkylene oxide under the action of a catalyst, wherein the inventor discloses a traditional Chinese patent document CN111378101A in Meng Yue, and the like, adopts a commercial, simple and efficient catalytic initiation system to catalyze and initiate the ternary polymerization reaction of propylene oxide, carbon dioxide and phthalic anhydride, successfully introduces an aromatic polyester structure with the content of 10-40% into polymethyl ethylene carbonate (PPC), and the product has good biodegradability, light transmittance, barrier property and the like through synthesizing and modifying the PPC, and is used for agricultural mulching films, food packaging bags, disposable medical materials and the like; however, because the glass transition temperature of PPC is low (30-40 ℃), it also has certain drawbacks in links of industrial processing, transportation, etc., and related researchers have also utilized various methods to increase the glass transition temperature, such as: ternary polymerization, crosslinking, blending with other polymers, inorganic fillers, organic compounding, and the like.
The prior patent document CN111378101A synthesizes the semi-aromatic polyester-polycarbonate copolymer polymer under certain reaction conditions by introducing aromatic anhydride as a reaction monomer and reacting with propylene oxide and carbon dioxide through the action of a catalyst, can effectively improve the glass transition temperature of the material and reduce the melt index of the material, and is very beneficial to subsequent processing and transportation; and the molecular weight and the distribution of the polymer product can be effectively improved by adding the polymerization auxiliary agent.
However, the existing market has some mature condensation devolatilization processes, which have certain limitations, such as difficulty in completely removing catalyst residues, complex process, high production cost and the like, and are not suitable for all PPC products. Under the condition of bulk polymerization process, propylene oxide is used as both monomer and solvent, and when the polymerization reaction is finished, the crude product contains 30% -70% of propylene oxide, and the part of raw materials need to be recovered to reduce the production cost. The residual propylene oxide can also cause the polymer to have strong pungent odor and harm human health. Notably, the formation of cyclic carbonates as by-products during the polymerization process is accompanied by the negative effect that the residues in the product have on the properties of the product, and therefore require complete removal.
Accordingly, there is a need for improvement and development in the art.
Disclosure of Invention
In order to solve the technical problems, the invention provides a condensing and devolatilizing device of a semi-aromatic polyester-polycarbonate copolymer, which can reduce the condensing and devolatilizing time after polymerization, obviously improve the condensing and devolatilizing efficiency, obviously improve the quality of PPC products and is suitable for all PPC products.
Meanwhile, the invention also provides a condensation devolatilization method of the semi-aromatic polyester-polycarbonate copolymer, which can greatly reduce the cost of PPC products, obviously reduce the negative influence of small molecule residues on the performance of the PPC products, obviously improve the quality of the PPC products and is suitable for all PPC products.
The technical scheme of the invention is as follows:
the semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization device comprises a polymerization reaction kettle, a glue solution storage tank, a washing coagulation devolatilization kettle, a conveying pump, a vibrating screen, a horizontal grinding machine and a horizontal spiral separator; the lower part of the polymerization reaction kettle is provided with a product outlet, and the upper part of the polymerization reaction kettle is provided with a gas outlet; the upper part of the glue solution storage tank is provided with a product inlet and a gas outlet, and the lower part of the glue solution storage tank is provided with a glue solution outlet; the product inlet of the glue solution storage tank is communicated to the product outlet of the polymerization reaction kettle through a corresponding pipeline; the lower part of the washing, condensing and devolatilizing kettle is provided with a glue solution inlet, and the upper part is provided with a product outlet and a gas outlet; the glue solution inlet of the washing, condensing and devolatilizing kettle is communicated to the glue solution outlet of the glue solution storage tank through a corresponding pipeline; the conveying pump is arranged on a pipeline which is communicated between a glue solution outlet of the glue solution storage tank and a glue solution inlet of the washing, condensing and devolatilizing kettle; the product outlet of the washing, condensing and devolatilizing kettle is communicated with a vibrating screen through a corresponding pipeline, the vibrating screen is communicated with a horizontal grinding machine through a corresponding pipeline, and the horizontal grinding machine is communicated with the inlet end of a horizontal spiral separator through a corresponding pipeline;
the middle part of the glue solution storage tank is provided with a liquid inlet which is used for adding 5-15wt% of water into the glue solution storage tank through a corresponding pipeline, and mixing the water with the glue solution in the glue solution storage tank to terminate the polymerization reaction;
at least two washing, condensing and devolatilizing kettles are connected in parallel between a glue solution storage tank and a vibrating screen, glue solution inlets of each washing, condensing and devolatilizing kettle are collected to corresponding pipelines through parallel pipelines and then communicated with a conveying pump, and product outlets of each washing, condensing and devolatilizing kettle are collected to corresponding pipelines through parallel pipelines and then communicated with inlet ends of the vibrating screen;
and the lower part of each washing, condensing and devolatilizing kettle is provided with a hot water inlet for injecting 60-90 ℃ hot water into the washing, condensing and devolatilizing kettle through corresponding pipelines so as to remove the propylene oxide component in the glue solution.
Further, in the above-mentioned semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus: three washing, condensing and devolatilizing kettles are connected in parallel between the glue solution storage tank and the vibrating screen.
Further, in the above-mentioned semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus, the capacity of the polymerization reactor was 30L, the capacity of the dope tank was 40L, and the capacity of each washing coagulation devolatilization reactor was 30L.
Further, in the above-mentioned coagulation devolatilization apparatus of a semiaromatic polyester-polycarbonate copolymer, a stirring device is provided in the polymerization reactor.
Further, in the above-mentioned coagulation devolatilization apparatus of a semiaromatic polyester-polycarbonate copolymer, a stirring device is provided in the dope tank.
Further, in the above-mentioned semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus, a stirring apparatus is provided in the washing coagulation devolatilization vessel.
Further, in the above-mentioned semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus, the grinding medium used in the horizontal grinder is ethanol at a temperature of 30.+ -. 10 ℃.
Further, in the above-mentioned semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus, the diameter of the pipe communicating with the glue solution inlet of each washing coagulation devolatilization kettle is 50-100 mm.
Further, in the above-mentioned semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus, the hot water at 60 to 90 ℃ contains 2 to 5wt% of a dispersing agent.
A method for condensing and devolatilizing a semi-aromatic polyester-polycarbonate copolymer, which adopts the condensing and devolatilizing device of the semi-aromatic polyester-polycarbonate copolymer, comprises the following steps:
A. adding 5-15wt% of water into the glue solution storage tank, and stirring and mixing with the crude product in the glue solution storage tank to terminate the polymerization reaction;
B. injecting hot water with the temperature of 60-90 ℃ containing 2-5wt% of dispersing agent into the washing, condensing and devolatilizing kettle to remove epoxypropane components in the glue solution; the flow rate of injecting hot water into the washing, condensing and devolatilizing kettle is regulated and controlled to be matched with the flow rate of pumping glue solution into the washing, condensing and devolatilizing kettle, so that the mass ratio of the water to the glue solution is controlled to be 95:5-80:20, and the residence time of the glue solution in the washing, condensing and devolatilizing kettle is longer than 30 minutes;
C. the grinding balls added into the horizontal grinding machine are ceramic balls, the diameter of each grinding ball is 1-5 cm, the amount of the added grinding balls accounts for 30% -60% of the volume of the horizontal grinding machine, and the particle size of the ground material is smaller than 5mm;
D. and (3) centrifugally separating the polymer from the ethanol by a horizontal screw separator to obtain a polymer containing 10-15 wt% of ethanol, and returning the separated ethanol to an ethanol storage tank for reuse.
According to the condensing and devolatilizing device and the condensing and devolatilizing method for the semi-aromatic polyester-polycarbonate copolymer, 5-15wt% of water is adopted to terminate the polymerization reaction, and then 60-90 ℃ hot water containing 2-5wt% of dispersing agent is adopted as a washing coagulant, so that propylene oxide serving as a reactant and a solvent is efficiently recovered, the condensing and devolatilizing time after polymerization can be reduced, the condensing and devolatilizing efficiency is obviously improved, the cost of a PPC product is greatly reduced, the negative influence of small molecular residues on the performance of the PPC product is obviously reduced, the quality of the PPC product is obviously improved, and the condensing and devolatilizing device and the condensing and devolatilizing method are applicable to all PPC products.
Drawings
The drawings described herein are for illustration purposes only and are not intended to limit the scope of the present disclosure in any way; the shapes and proportional sizes of the components in the drawings are only illustrative, and are not intended to limit the shapes and proportional sizes of the components of the present invention in particular, so as to assist in understanding the present invention; those skilled in the art with access to the teachings of the present invention can select a variety of possible shapes and scale sizes to practice the present invention as the case may be.
FIG. 1 is a schematic structural view of an embodiment of a coagulation devolatilization apparatus of a semiaromatic polyester-polycarbonate copolymer of the present invention;
FIG. 2 is a nuclear magnetic resonance spectrum of each component of a sample obtained in example one of the coagulation devolatilization method of the semiaromatic polyester-polycarbonate copolymer of the present invention;
the reference numerals in the figures are summarized: a polymerization reaction kettle 1, a product outlet 1-1, a gas outlet 1-2, a glue solution storage tank 2, a product inlet 2-1, a gas outlet 2-2, a liquid inlet 2-3, a glue solution outlet 2-4, a washing coagulation devolatilization kettle 3, a glue solution inlet 3-1, a gas outlet 3-2, a hot water (washing coagulant) inlet 3-3, a product outlet 3-4, a vibrating screen 4, a horizontal grinding machine 5 and a horizontal spiral separator 6, a next processing unit 7, a conveying pump 8, and pipelines (9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22).
Detailed Description
The following detailed description and examples of the invention are presented in conjunction with the drawings, and the described examples are intended to illustrate the invention and not to limit the invention to the specific embodiments.
As shown in fig. 1, fig. 1 is a schematic structural view of an embodiment of a coagulation devolatilization apparatus of a semiaromatic polyester-polycarbonate copolymer of the present invention, which comprises a polymerization reaction vessel 1, a glue solution storage tank 2, a washing coagulation devolatilization vessel 3, a transfer pump 8, a vibrating screen 4, a horizontal grinder 5 and a horizontal screw separator 6; wherein, the lower part of the polymerization reaction kettle 1 is provided with a product outlet 1-1, the upper part is provided with a gas outlet 1-2, and the gas outlet 1-2 is used for emptying under abnormal conditions; the upper part of the glue solution storage tank 2 is provided with a product inlet 2-1 and a gas outlet 2-2, and the lower part is provided with a glue solution outlet 2-4; the product inlet 2-1 of the glue solution storage tank 2 is communicated with the product outlet 1-1 of the polymerization reaction kettle 1 through a corresponding pipeline 9; the lower part of the washing, condensing and devolatilizing kettle 3 is provided with a glue solution inlet 3-1 and a hot water inlet 3-3, and the upper part is provided with a product outlet 3-4 and a gas outlet 3-2; the glue solution inlet 3-1 of the washing coagulation devolatilization kettle 3 is communicated with the glue solution outlet 2-4 of the glue solution storage tank 2 through a corresponding pipeline 12; hot water enters the washing, condensing and devolatilizing kettle 3 from a hot water inlet 3-3 through a pipeline 13, and a conveying pump 8 is arranged on a pipeline 12 which is communicated between a glue solution outlet 2-4 of a glue solution storage tank 2 and a glue solution inlet 3-1 of the washing, condensing and devolatilizing kettle 3; the product outlet 3-4 of the washing, condensing and devolatilizing kettle 3 is communicated with the inlet end of the vibrating screen 4 through corresponding pipelines (15 and 16), the outlet end of the vibrating screen 4 is communicated with the inlet end of the horizontal grinding machine 5, the outlet end of the horizontal grinding machine 5 is communicated with the inlet end of the horizontal spiral separator 6, and the outlet end of the horizontal spiral separator 6 is communicated with the next treatment unit 7.
Preferably, the polymerization reaction kettle 1, the glue solution storage tank 2 and the washing, condensing and devolatilizing kettle 3 are respectively provided with respective stirring devices, so that better volatilization functions of the polymerization reaction kettle 1, the glue solution storage tank 2 and the washing, condensing and devolatilizing kettle 3 can be realized.
Unlike the coagulation devolatilizer of the prior art, the coagulation devolatilizer of the semiaromatic polyester-polycarbonate copolymer of the present invention is improved in that: on the one hand, the middle part of the glue solution storage tank 2 is provided with a liquid inlet 2-3 which is used for adding water accounting for 5-15wt% of the total amount of the glue solution into the glue solution storage tank 2 through a corresponding pipeline 11, stirring and mixing the water and a crude product in the glue solution storage tank 2 to stop the polymerization reaction, and enabling partial monomer solvents such as propylene oxide monomers to volatilize into gas to enter a corresponding pipeline 10 from a gas outlet 2-2, so that the obtained glue solution is sprayed into a washing coagulation devolatilization kettle 3 from a glue solution inlet 3-1 through a corresponding pipeline 12 from a glue solution outlet 2-4 under the action of a conveying pump 8; on the other hand, at least two washing and condensing devolatilization kettles 3 (such as three washing and condensing devolatilization kettles 3 shown in the embodiment of fig. 1) are connected in parallel between a glue solution storage tank 2 and a vibrating screen 4, a glue solution inlet 3-1 of each washing and condensing devolatilization kettle 3 is collected to a corresponding pipeline 12 through a parallel pipeline and then is communicated with a conveying pump 8, and a product outlet 3-4 of each washing and condensing devolatilization kettle 3 is collected to a corresponding pipeline 16 through a parallel pipeline 15 and then is communicated with an inlet end of a horizontal spiral separator 6 through the vibrating screen 4 and a horizontal grinder 5; and the lower part of each washing coagulation devolatilization kettle 3 is provided with a washing coagulant inlet 3-3 for injecting hot water containing 2-5wt% of dispersing agent into the washing coagulation devolatilization kettle 3 through a corresponding pipeline, volatilizing propylene oxide remained in the glue solution into gas to the greatest extent, and entering a corresponding pipeline 14 from a gas outlet 3-2, and washing out catalyst and cyclic carbonate and other component parts, thereby obtaining a semi-aromatic polyester-polycarbonate copolymer bulk solid suspension, separating the hot water from the polymer by utilizing a vibrating screen 5, then adding ethanol into a horizontal grinder 5 to wash the water, grinding the polymer into smaller particles, and separating the ethanol from the polymer through a horizontal spiral separator 6 to finally obtain the semi-aromatic polyester-polycarbonate copolymer powdery solid.
Aiming at the physical characteristics of the semi-aromatic polyester-polycarbonate copolymer, the condensation devolatilization device creatively adopts the steps of stirring and mixing 5-15wt% of water with the glue solution in the glue solution storage tank 2 to terminate the polymerization reaction, taking hot water containing 2-5wt% of dispersing agent at 60-90 ℃ as a washing coagulant, and removing the components such as low boiling monomer propylene oxide (34 ℃) left in the glue solution, a catalyst, cyclic carbonate and the like in the washing condensation devolatilization kettle 3 as much as possible, and simultaneously combining a parallel structure formed by at least two washing condensation devolatilization kettles 3, so that the condensation devolatilization time can be greatly shortened, the condensation devolatilization efficiency can be obviously improved, the quality of PPC products can be obviously improved, and the device is applicable to all PPC products.
Preferably, hot water of 60-90 ℃ which is 5-15 wt% of the total amount of the glue solution is added into the glue solution storage tank 2 from the liquid inlet 2-3 of the glue solution storage tank 2 through the corresponding pipeline 11, more propylene oxide monomer volatilizes into gas by utilizing the pressure of the glue solution storage tank 2, and enters the corresponding pipeline 10 from the gas outlet 2-2, so that the glue solution can be obtained more rapidly.
The glue solution in the glue solution storage tank 2 comprises semi-aromatic polyester-polycarbonate copolymer, propylene oxide, cyclic carbonate, catalyst, cocatalyst and branching agent, wherein the catalyst, cocatalyst and branching agent are well known in the art and are not described herein.
Preferably, the horizontal mill 5 is a ball mill and the milling medium is ethanol at a temperature of 30.+ -. 10 ℃ and the bulk polymer hardens on cooling as the semiaromatic polyester-polycarbonate copolymer enters the horizontal mill, thereby facilitating the milling of the semiaromatic polyester-polycarbonate copolymer into a powdered solid.
Preferably, the diameter of the pipeline 12 communicated with the glue solution inlet 3-1 of each washing, condensing and devolatilizing kettle 3 is 50-100 mm, the flow rate of injecting hot water at 60-90 ℃ from the hot water inlet 3-3 into the washing, condensing and devolatilizing kettle 3 is regulated and controlled to be matched with the flow rate of pumping glue solution into the washing, condensing and devolatilizing kettle 3 through the conveying pump 8, so that the obtained semi-aromatic polyester-polycarbonate copolymer blocky solid suspension has better flowability and higher apparent density, is more beneficial to solid-liquid separation of the vibrating screen 4, and is also beneficial to grinding of the horizontal grinding machine 5.
Based on the above-mentioned semi-aromatic polyester-polycarbonate copolymer coagulation and devolatilization device, the invention also provides a semi-aromatic polyester-polycarbonate copolymer coagulation and devolatilization method, which mainly comprises the following steps:
A. adding 5-15wt% of water into the glue solution storage tank, and stirring and mixing with the crude product in the glue solution storage tank to terminate the polymerization reaction;
B. injecting hot water with the temperature of 60-90 ℃ containing 2-5wt% of dispersing agent into the washing, condensing and devolatilizing kettle to remove epoxypropane components in the glue solution; the flow rate of injecting hot water into the washing, condensing and devolatilizing kettle is regulated and controlled to be matched with the flow rate of pumping glue solution into the washing, condensing and devolatilizing kettle, so that the mass ratio of the water to the glue solution is controlled to be 95:5-80:20, and the residence time of the glue solution in the washing, condensing and devolatilizing kettle is longer than 30 minutes;
C. the grinding balls added into the horizontal grinding machine are ceramic balls, the diameter of each grinding ball is 1-5 cm, the amount of the added grinding balls accounts for 30% -60% of the volume of the horizontal grinding machine, and the particle size of the ground material is smaller than 5mm;
D. and (3) centrifugally separating the polymer from the ethanol by a horizontal screw separator to obtain a polymer containing 10-15 wt% of ethanol, and returning the separated ethanol to an ethanol storage tank for reuse.
The condensation devolatilization method of the semi-aromatic polyester-polycarbonate copolymer greatly reduces the cost of PPC products, obviously reduces the negative influence of small molecular residues on the performance of the PPC products, obviously improves the quality of the PPC products, and is suitable for all PPC products; the production process is simpler, is more suitable for automatic control, can continuously perform condensation and devolatilization operation, and can fully utilize material energy sources; the adopted condensing devolatilization device is basically a pressurized closed container and a pipeline, is not in contact with ambient air at all, is basically free from gas phase evacuation (namely, is collected by a condensing system) in the operation process, does not need cleaning, and has the advantages of complete product ash removal and devolatilization, little solid-liquid waste, and meeting the raw material use requirements of the related fields; meanwhile, the industrialized production cost is lower, and the industrialized process basically meets the green chemical requirement.
In the embodiment 1, taking a 30L polymerization reaction kettle 1, a 40L glue solution storage tank 2 and three parallel 30L washing, condensing and devolatilizing kettles 3 as examples, the diameter of a pipeline 13 communicated with a glue solution inlet 3-1 of each washing, condensing and devolatilizing kettle 3 is 50mm, the content of epoxy propane in reaction solution after polymerization reaction of the polymerization reaction kettle 1 is 40wt% and the content of cyclic carbonate is 10wt%, the reaction solution is injected into the glue solution storage tank 2, meanwhile, 85 ℃ hot water which is equivalent to 10wt% of the reaction solution is added to terminate the reaction to obtain glue solution, and then the glue solution is injected into the washing, condensing and devolatilizing kettle 3 through a glue solution pump 8, and meanwhile, 85 ℃ hot water is injected; after the coagulation devolatilization device of the semi-aromatic polyester-polycarbonate copolymer is adopted for coagulation devolatilization, the content of propylene oxide in the obtained powdery solid of the semi-aromatic polyester-polycarbonate copolymer is reduced to 0.2 weight percent, and the content of cyclic carbonate is reduced to 1.2 weight percent; after drying, the mixture was dissolved in methylene chloride, and no turbidity was observed during the washing by ethanol extraction, i.e., no significant (oligomer and catalyst) residues were observed.
Meanwhile, the invention also adopts nuclear magnetic resonance spectroscopy (Nuclear Magnetic Resonance Spectroscopy, called NMR for short) for researching the absorption of atomic check Radio frequency radiation (Radio-frequency Radiation) to analyze and verify the composition and structure of the semi-aromatic polyester-polycarbonate copolymer powder obtained in the example 1, and is shown in the combination of fig. 2, wherein, fig. 2 is the nuclear magnetic resonance spectrum of the material obtained after the condensation devolatilization in the example 1, D represents the semi-aromatic polyester-polycarbonate copolymer, E represents the cyclic carbonate, and F represents the propylene oxide; as can also be seen from the verification results of FIG. 2, after the coagulation devolatilization apparatus of the semi-aromatic polyester-polycarbonate copolymer of the present invention is used for coagulation devolatilization, the content of both the propylene oxide component and the cyclic carbonate component is significantly reduced, and particularly the propylene oxide component as a monomer and a solvent has been substantially removed from the PPC product.
Example 2 was different from example 1 in that the propylene oxide content in the reaction liquid after completion of the polymerization reaction in the polymerization reactor 1 was 45wt% and the cyclic carbonate content was 9wt%; after the coagulation devolatilization device of the semi-aromatic polyester-polycarbonate copolymer is adopted for coagulation devolatilization, the content of propylene oxide in the obtained powdery solid of the semi-aromatic polyester-polycarbonate copolymer is reduced to 0.3 weight percent, and the content of cyclic carbonate is reduced to 1.0 weight percent; after drying, the obtained product was dissolved in methylene chloride, and no turbidity was observed even when the obtained product was washed by ethanol extraction, i.e., no significant (oligomer and catalyst) residue was observed.
Example 3, unlike example 1, the propylene oxide content in the reaction liquid after completion of the polymerization reaction in the polymerization reactor 1 was 50wt% and the cyclic carbonate content was 11wt%; after the coagulation devolatilization device of the semi-aromatic polyester-polycarbonate copolymer is adopted for coagulation devolatilization, the content of propylene oxide in the obtained powdery solid of the semi-aromatic polyester-polycarbonate copolymer is reduced to 0.4 weight percent, and the content of cyclic carbonate is reduced to 1.3 weight percent; after drying, the mixture was dissolved in methylene chloride, and the mixture was washed with ethanol, and was free from turbidity, i.e., no significant precipitation of residues (oligomers and catalyst) was observed.
As can be seen from the data of the above three examples, with the gradual increase of the propylene oxide content and the cyclic carbonate content in the reaction liquid of the polymerization reactor 1, the propylene oxide content and the cyclic carbonate content in the powdery solid of the obtained semiaromatic polyester-polycarbonate copolymer were not significantly increased after the coagulation devolatilization by using the coagulation devolatilization apparatus of the semiaromatic polyester-polycarbonate copolymer of the present invention, which indicates that the coagulation devolatilization apparatus and the method of the semiaromatic polyester-polycarbonate copolymer of the present invention have an efficient removal effect for both the propylene oxide component and the cyclic carbonate component in the semiaromatic polyester-polycarbonate copolymer.
It should be understood that the foregoing description is only of the preferred embodiments of the present invention and is not intended to limit the technical solutions of the present invention, and it should be understood that the foregoing may be added, substituted, altered or modified within the spirit and principle of the present invention by those skilled in the art, and all such added, substituted, altered or modified embodiments fall within the scope of the appended claims.

Claims (10)

1. The semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization device is characterized by comprising a polymerization reaction kettle, a glue solution storage tank, a washing coagulation devolatilization kettle, a conveying pump, a vibrating screen, a horizontal grinding machine and a horizontal screw separator; the lower part of the polymerization reaction kettle is provided with a product outlet, and the upper part of the polymerization reaction kettle is provided with a gas outlet; the upper part of the glue solution storage tank is provided with a product inlet and a gas outlet, and the lower part of the glue solution storage tank is provided with a glue solution outlet; the product inlet of the glue solution storage tank is communicated to the product outlet of the polymerization reaction kettle through a corresponding pipeline; the lower part of the washing, condensing and devolatilizing kettle is provided with a glue solution inlet and a hot water inlet, and the upper part is provided with a product outlet and a gas outlet; the glue solution inlet of the washing, condensing and devolatilizing kettle is communicated to the glue solution outlet of the glue solution storage tank through a corresponding pipeline; the conveying pump is arranged on a pipeline which is communicated between a glue solution outlet of the glue solution storage tank and a glue solution inlet of the washing, condensing and devolatilizing kettle; the product outlet of the washing, condensing and devolatilizing kettle is communicated with a vibrating screen through a corresponding pipeline, the vibrating screen is communicated with a horizontal grinding machine through a corresponding pipeline, and the horizontal grinding machine is communicated with the inlet end of a horizontal spiral separator through a corresponding pipeline;
the middle part of the glue solution storage tank is provided with a liquid inlet for adding 5-15 wt% of water into the glue solution storage tank through corresponding pipelines, and mixing the water with the glue solution in the glue solution storage tank to terminate the polymerization reaction;
at least two washing, condensing and devolatilizing kettles are connected in parallel between a glue solution storage tank and a vibrating screen, glue solution inlets of each washing, condensing and devolatilizing kettle are collected to corresponding pipelines through parallel pipelines and then communicated with a conveying pump, and product outlets of each washing, condensing and devolatilizing kettle are collected to corresponding pipelines through parallel pipelines and then communicated with inlet ends of the vibrating screen;
the lower part of each washing, condensing and devolatilizing kettle is provided with a hot water inlet for injecting 60-90 ℃ hot water into the washing, condensing and devolatilizing kettle through a corresponding pipeline so as to remove the propylene oxide component in the glue solution;
the polycarbonate is PPC.
2. The semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus as claimed in claim 1, wherein: three washing, condensing and devolatilizing kettles are connected in parallel between the glue solution storage tank and the vibrating screen.
3. The semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus as claimed in claim 1, wherein: the capacity of the polymerization reaction kettle is 30L, the capacity of the glue solution storage tank is 40L, and the capacity of each washing, condensing and devolatilizing kettle is 30L.
4. The semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus as claimed in claim 1, wherein: and a stirring device is arranged in the polymerization reaction kettle.
5. The semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus as claimed in claim 1, wherein: and a stirring device is arranged in the glue solution storage tank.
6. The semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus as claimed in claim 1, wherein: and a stirring device is arranged in the washing, condensing and devolatilizing kettle.
7. The semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus as claimed in claim 1, wherein: the grinding medium adopted by the horizontal grinder is ethanol with the temperature of 30+/-10 ℃.
8. The semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus as claimed in claim 1, wherein: the diameter of the pipeline communicated with the glue solution inlet of each washing, condensing and devolatilizing kettle is between 50 and 100 mm.
9. The semi-aromatic polyester-polycarbonate copolymer coagulation devolatilization apparatus as claimed in claim 1, wherein: the hot water at 60-90 ℃ contains 2-5wt% of dispersing agent.
10. A method for condensing and devolatilizing the semiaromatic polyester-polycarbonate copolymer, using the apparatus for condensing and devolatilizing the semiaromatic polyester-polycarbonate copolymer according to any of claims 1 to 9, characterized by comprising the steps of:
A. adding 5-15 wt% of water into the glue solution storage tank, and stirring and mixing with the crude product in the glue solution storage tank to terminate the polymerization reaction;
B. injecting hot water with the temperature of 60-90 ℃ containing 2-5wt% of dispersing agent into the washing coagulation devolatilization kettle to remove epoxypropane component in the glue solution; the flow rate of injecting hot water into the washing, condensing and devolatilizing kettle is regulated and controlled to be matched with the flow rate of pumping glue solution into the washing, condensing and devolatilizing kettle, so that the mass ratio of the water to the glue solution is controlled to be 95:5-80:20, and the residence time of the glue solution in the washing, condensing and devolatilizing kettle is longer than 30 minutes;
C. the grinding balls added into the horizontal grinding machine are ceramic balls, the diameter of each grinding ball is 1-5 cm, the amount of the added grinding balls accounts for 30% -60% of the volume of the horizontal grinding machine, and the particle size of the ground material is smaller than 5mm;
D. the horizontal screw separator centrifugally separates the polymer from the ethanol to obtain a polymer containing 10-15 wt% of ethanol, and the separated ethanol is returned to the ethanol storage tank for reuse.
CN202110266157.9A 2021-03-11 2021-03-11 Condensation devolatilization device and method for semi-aromatic polyester-polycarbonate copolymer Active CN112898552B (en)