CN116445857A - High-strength composite coating, preparation method and application thereof - Google Patents

High-strength composite coating, preparation method and application thereof Download PDF

Info

Publication number
CN116445857A
CN116445857A CN202310483332.9A CN202310483332A CN116445857A CN 116445857 A CN116445857 A CN 116445857A CN 202310483332 A CN202310483332 A CN 202310483332A CN 116445857 A CN116445857 A CN 116445857A
Authority
CN
China
Prior art keywords
layer
composite coating
target
strength composite
nano
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN202310483332.9A
Other languages
Chinese (zh)
Inventor
孙德恩
李茂丽
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Southwest University
Original Assignee
Southwest University
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Southwest University filed Critical Southwest University
Priority to CN202310483332.9A priority Critical patent/CN116445857A/en
Publication of CN116445857A publication Critical patent/CN116445857A/en
Pending legal-status Critical Current

Abstract

A high-strength composite coating relates to the technical field of surface engineering, and comprises the following components: the substrate, the transition layer and the functional layer are sequentially arranged; wherein the matrix is 4Cr5MoV1Si alloy, the transition layer is metal Cr, and the functional layer is formed by alternately depositing a SiN nano layer and a CrSiN nano layer for multiple times; the invention also provides a preparation method of the high-strength composite coating, which comprises the following steps: pretreatment of a matrix, glow cleaning, preparation of a transition layer and preparation of a functional layer; the invention also provides application of the high-strength composite coating on an aluminum alloy die casting die; the coating has the capability of resisting rapid temperature rise and fall impact, and also has high hardness and high wear resistance.

Description

一种高强度复合涂层、制备方法及其应用A kind of high-strength composite coating, preparation method and application thereof

技术领域technical field

本发明涉及表面工程技术领域,具体涉及一种高强度复合涂层、制备方法及其应用。The invention relates to the technical field of surface engineering, in particular to a high-strength composite coating, a preparation method and an application thereof.

背景技术Background technique

铝合金压铸是一种通过高压方式将熔融铝合金液体快速挤压到精密金属模腔中,并随后使之凝固成形的铸造工艺。压铸模是压铸工艺中的重要部件,其工作性能和使用寿命对产品的质量和成本具有较大的影响;压铸模是一种将熔化的金属在压力作用下成形的模具,具有承受高冲击载荷、长工作时间、高工作温度和高交变应力的作用,这就要求模具材质具有良好的高温强度和耐热疲劳能力。Aluminum alloy die-casting is a casting process that rapidly extrudes molten aluminum alloy liquid into a precision metal mold cavity by high pressure, and then solidifies it into shape. The die-casting mold is an important part in the die-casting process, and its working performance and service life have a great influence on the quality and cost of the product; the die-casting mold is a mold that forms molten metal under pressure, and has the ability to withstand high impact loads , long working time, high working temperature and high alternating stress, which requires the mold material to have good high temperature strength and thermal fatigue resistance.

铝合金压铸模在工作过程中,与铝合金的长时间直接接触会发生腐蚀,而且压铸模在使用过程中多次承受金属加热和冷却介质冷却,容易导致热疲劳,还会引起压铸模的开裂。为了改善这种情况,现有采用的方式一种是通过改变模具的合金组成,来改善其性能,延长其使用寿命;另一种是通过表面强化来改善压铸模的强度和耐磨性,延长热裂纹的潜伏时间,避免热裂纹的蔓延,以达到延长压铸模寿命的目的,而且通过表面渗碳、渗氮等工艺,还能有效降低模具的磨损,提高耐热性。During the working process, the aluminum alloy die-casting mold will be corroded when it is in direct contact with the aluminum alloy for a long time, and the die-casting mold is repeatedly subjected to metal heating and cooling medium cooling during use, which will easily lead to thermal fatigue and cracking of the die-casting mold . In order to improve this situation, one of the existing methods is to improve its performance and prolong its service life by changing the alloy composition of the mold; the other is to improve the strength and wear resistance of the die-casting mold through surface strengthening, prolonging the The latent time of hot cracks can avoid the spread of hot cracks to achieve the purpose of prolonging the life of die-casting molds, and through surface carburizing, nitriding and other processes, it can also effectively reduce mold wear and improve heat resistance.

在公开号为CN109609905A的中国发明中,提供了一种高硬度抗冲耐磨复合涂层、制备方法及应用,其中通过在钛合金表面制备由Cr粘结层、Cr/CrSiN工作层构成的复合防护涂层,显著改善钛合金的硬度、耐磨及抗冲蚀性,延长使用寿命;但是其中Cr/CrSiN工作层由依次沉积的Cr层、CrSiN层组成,而且Cr层为金属相,CrSiN层为陶瓷相,两者之间的结合力不是很好,在磨损和侵蚀等反复交变应力条件下会发生剥离情况,导致涂层的硬度较低,影响涂层的使用寿命。In the Chinese invention with the publication number CN109609905A, a high-hardness impact-resistant and wear-resistant composite coating, preparation method and application are provided, wherein a composite coating consisting of a Cr bonding layer and a Cr/CrSiN working layer is prepared on the surface of a titanium alloy Protective coating, which significantly improves the hardness, wear resistance and erosion resistance of titanium alloys, and prolongs the service life; however, the Cr/CrSiN working layer is composed of a Cr layer and a CrSiN layer deposited in sequence, and the Cr layer is a metal phase, and the CrSiN layer It is a ceramic phase, the bonding force between the two is not very good, and peeling will occur under repeated alternating stress conditions such as wear and erosion, resulting in low hardness of the coating and affecting the service life of the coating.

发明内容Contents of the invention

针对现有技术中所存在的不足,本发明提供了一种高强度复合涂层、制备方法及其应用,其解决了现有技术中存在的涂层的结合力较差、硬度较低的问题。Aiming at the deficiencies in the prior art, the present invention provides a high-strength composite coating, a preparation method and its application, which solves the problems of poor bonding and low hardness of the coating existing in the prior art .

一种高强度复合涂层,包括:A high-strength composite coating comprising:

依次设置的基体、过渡层以及功能层;Substrate, transition layer and functional layer arranged in sequence;

其中所述基体为4Cr5MoV1Si合金,所述过渡层为金属Cr,所述功能层为SiN纳米层和CrSiN纳米层多次交替沉积而成。Wherein the substrate is 4Cr5MoV1Si alloy, the transition layer is metallic Cr, and the functional layer is formed by alternately depositing SiN nano-layers and CrSiN nano-layers multiple times.

优选地,所述过渡层厚度为150nm~200nm。Preferably, the thickness of the transition layer is 150nm-200nm.

优选地,所述功能层的厚度为670nm~750nm,其中SiN纳米层与CrSiN纳米层的调制周期比为2:1。Preferably, the thickness of the functional layer is 670nm-750nm, wherein the modulation period ratio of the SiN nanolayer to the CrSiN nanolayer is 2:1.

优选地,SiN纳米层和CrSiN纳米层交替沉积的次数为1~15次。Preferably, the number of alternate depositions of SiN nano-layers and CrSiN nano-layers is 1-15 times.

本发明还提供了一种高强度复合涂层的制备方法,包括以下步骤:The present invention also provides a method for preparing a high-strength composite coating, comprising the following steps:

(1)对基体进行喷砂、打磨、抛光、清洗以及干燥后备用;(1) Sandblasting, grinding, polishing, cleaning and drying the substrate for subsequent use;

(2)将处理完成基体放入超声波清洗机中,在15~30kHZ的频率下使用清洗液进行连续清洗15分钟;(2) Put the processed substrate into an ultrasonic cleaning machine, and use cleaning solution to clean continuously for 15 minutes at a frequency of 15-30kHZ;

(3)将清洗后的基体放进多靶磁控溅射镀膜机的真空室内,抽真空至9.0×10-4Pa,然后向其中通入气流量为40sccm的Ar气,此时维持真空室内真空度为3Pa,最后用溅射功率密度为10~15W/cm2的射频电源对基体进行离子轰击30min,以对基体进行辉光清洗;(3) Put the cleaned substrate into the vacuum chamber of a multi-target magnetron sputtering coating machine, evacuate to 9.0×10 -4 Pa, and then pass Ar gas with a gas flow rate of 40 sccm into it, and maintain the vacuum chamber at this time. The degree of vacuum is 3 Pa, and finally, the substrate is bombarded with ions for 30 minutes with a radio frequency power source with a sputtering power density of 10-15W/cm 2 to perform glow cleaning on the substrate;

(4)过渡层的制备:开启Cr靶,逐渐调高溅射电流,使Cr靶起辉,将Cr靶的溅射功率密度调至10~15W/cm2,进行过渡层Cr层的沉积,沉积时间为10min;(4) Preparation of the transition layer: turn on the Cr target, gradually increase the sputtering current to make the Cr target glow, adjust the sputtering power density of the Cr target to 10-15W/cm 2 , and deposit the Cr layer of the transition layer. Deposition time is 10min;

(5)功能层的制备:向真空室内通入流量为40sccm的N2,在Ar-N2的混合环境下,交替地开启Si靶材与Cr靶材前面的挡板,溅射沉积纳米级的多层膜,该多层膜是由多个SiN纳米层和CrSiN纳米层交替堆叠而成,同时调节Si靶材和Cr靶材的溅射功率密度和沉积时间,以控制SiN纳米层和CrSiN纳米层的调制周期。(5) Preparation of the functional layer: N 2 with a flow rate of 40 sccm is passed into the vacuum chamber, and in the mixed environment of Ar-N 2 , the baffles in front of the Si target and the Cr target are alternately opened, and the nano-scale The multilayer film is composed of multiple SiN nanolayers and CrSiN nanolayers stacked alternately, and the sputtering power density and deposition time of the Si target and the Cr target are adjusted at the same time to control the SiN nanolayer and CrSiN Modulation period of the nanolayer.

优选地,步骤(2)中的清洗液包括丙酮和无水乙醇。Preferably, the cleaning solution in step (2) includes acetone and absolute ethanol.

优选地,步骤(5)中SiN纳米层和CrSiN纳米层的溅射功率密度均为10~15W/cm2。Preferably, the sputtering power density of the SiN nano-layer and the CrSiN nano-layer in step (5) is both 10-15 W/cm 2 .

优选地,步骤(5)中SiN纳米层的沉积时间为2.5~40min。Preferably, the deposition time of the SiN nano-layer in step (5) is 2.5-40 min.

优选地,步骤(5)中CrSiN纳米层的沉积时间为5~80min。Preferably, the deposition time of the CrSiN nano-layer in step (5) is 5-80 min.

本发明还提供了一种高强度复合涂层在铝合金压铸模具上的应用。The invention also provides the application of a high-strength composite coating on an aluminum alloy die-casting mold.

相比于现有技术,本发明具有如下有益效果:Compared with the prior art, the present invention has the following beneficial effects:

1、所得的高强度复合涂层在不影响铝合金压铸模具机械结构精度的条件下,具有耐快速升降温冲击的能力,同时还具有高硬度和高耐磨性能;1. The obtained high-strength composite coating has the ability to withstand the impact of rapid temperature rise and fall without affecting the mechanical structure accuracy of the aluminum alloy die-casting mold, and also has high hardness and high wear resistance;

2、其中CrSiN纳米层作为顶层,属于陶瓷结构,具有高硬度、良好的高温红硬性,且摩擦系数低,与液态铝的不浸润性好,有好的脱模性,且较高的Cr含量使得在高温下涂层表面可形成一层稳定致密的氧化膜,提高涂层的抗高温氧化性能;2. Among them, the CrSiN nano-layer is used as the top layer, which belongs to the ceramic structure, has high hardness, good high-temperature red hardness, and low friction coefficient, good non-wetting property with liquid aluminum, good mold release, and high Cr content A stable and dense oxide film can be formed on the surface of the coating at high temperature, which improves the high temperature oxidation resistance of the coating;

3、SiN是一种重要的结构陶瓷材料,本身硬度大、润滑性好、耐磨损,具有高温抗氧化性,且抵抗冷热冲击,在空气中加热到1000℃以上,急剧冷却再急剧加热,也不会破裂;3. SiN is an important structural ceramic material. It has high hardness, good lubricity, wear resistance, high temperature oxidation resistance, and resistance to cold and heat shock. It is heated to above 1000 °C in the air, cooled rapidly and then heated rapidly , will not break;

4、SiN/CrSiN多层膜结构属于“陶瓷-陶瓷”多层膜结构,可有效调节涂层的硬度和耐腐蚀性,且减少了在磨损和侵蚀等反复交变应力条件下涂层剥离的概率;4. The SiN/CrSiN multilayer film structure belongs to the "ceramic-ceramic" multilayer film structure, which can effectively adjust the hardness and corrosion resistance of the coating, and reduce the risk of coating peeling off under repeated alternating stress conditions such as wear and erosion. probability;

5、采用SiN/CrSiN纳米多层结构涂层,使层与层之间具有良好的结合力,由于界面交互作用,使涂层具有超高硬度,高温下可以阻碍涂层元素扩散,提高涂层的抗高温氧化性;除此之外,由于SiN和CrSiN的晶格结构不同,微裂纹不会迅速延伸穿透整个涂层,可实现模具在长期使用过程中的防护。5. The SiN/CrSiN nano-layer structure coating is used to make the layers have good bonding force. Due to the interface interaction, the coating has ultra-high hardness, which can hinder the diffusion of coating elements at high temperatures and improve the coating quality. Excellent high temperature oxidation resistance; In addition, due to the different lattice structures of SiN and CrSiN, microcracks will not quickly extend and penetrate the entire coating, which can realize the protection of the mold during long-term use.

本发明的其它优点、目标和特征将部分通过下面的说明体现,部分还将通过对本发明的研究和实践而为本领域的技术人员所理解。Other advantages, objectives and features of the present invention will partly be embodied through the following descriptions, and partly will be understood by those skilled in the art through the research and practice of the present invention.

附图说明Description of drawings

图1为本发明高强度复合涂层的结构示意图。Figure 1 is a schematic structural view of the high-strength composite coating of the present invention.

图2为调制周期为Λ=45nm,90nm,180nm下高强度复合涂层的SEM表面形貌。Fig. 2 is the SEM surface morphology of the high-strength composite coating under the modulation periods of Λ=45nm, 90nm, and 180nm.

具体实施方式Detailed ways

为了使本发明实现的技术手段、创作特征、达成目的与作用更加清楚及易于了解,下面结合附图和具体实施方式对本发明作进一步阐述:In order to make the technical means, creative features, goals and functions achieved by the present invention clearer and easier to understand, the present invention will be further elaborated below in conjunction with the accompanying drawings and specific embodiments:

实施例1Example 1

选择合金成分为4Cr5MoV1Si,尺寸为600×260×150mm的铝合金压铸模具作为基体,经喷砂、打磨、抛光、清洗、干燥后备用。An aluminum alloy die-casting mold with an alloy composition of 4Cr5MoV1Si and a size of 600×260×150mm was selected as the substrate, and it was sandblasted, polished, polished, cleaned and dried for later use.

将处理好的基体放入超声波清洗机中,按15kHz的频率用丙酮和无水乙醇连续清洗15分钟,将清洗后的基体放进多靶磁控溅射镀膜机的真空室内,随后抽真空至9.0×10- 4Pa,然后向其中通入气流量为40sccm的Ar气,此时维持真空室内真空度为3Pa,最后用溅射功率密度为10W/cm2的射频电源对基体进行离子轰击30min,以对基体进行辉光清洗;辉光清洗完成后,开启Cr靶,逐渐调高溅射电流,使Cr靶起辉,将Cr靶的溅射功率密度调至10W/cm2,进行过渡层Cr层的沉积,沉积时间为10min。Put the processed substrate into an ultrasonic cleaning machine, clean it continuously with acetone and absolute ethanol for 15 minutes at a frequency of 15 kHz, put the cleaned substrate into the vacuum chamber of a multi-target magnetron sputtering coating machine, and then evacuate to 9.0×10 - 4 Pa, and then pass Ar gas with a gas flow rate of 40 sccm into it. At this time, maintain the vacuum degree of the vacuum chamber at 3 Pa, and finally use a radio frequency power supply with a sputtering power density of 10W/cm 2 to bombard the substrate with ions for 30 minutes , to perform glow cleaning on the substrate; after the glow cleaning is completed, turn on the Cr target, gradually increase the sputtering current to make the Cr target glow, adjust the sputtering power density of the Cr target to 10W/cm 2 , and carry out the transition layer For the deposition of the Cr layer, the deposition time is 10 min.

向真空室内通入气流量为40sccm的N2,在Ar-N2的混合气氛中交替打开Si靶和Cr靶的挡板,在溅射沉积过程中不改变Si靶和Cr靶的溅射功率,而通过控制两个靶材前面挡板的开闭来控制所需沉积的涂层以及Si靶和Cr靶在基体上的沉积时间,以此来获得所需厚度的SiN纳米层和CrSiN纳米层,其中SiN以10W/cm2的溅射功率沉淀2.5min,CrSiN以10W/cm2的溅射功率沉淀5min,设置调制周期为Λ=45nm,得到厚度约为670nm的SiN/CrSiN纳米多层薄膜。Introduce N 2 with a gas flow rate of 40 sccm into the vacuum chamber, open the baffles of the Si target and the Cr target alternately in the Ar-N 2 mixed atmosphere, and do not change the sputtering power of the Si target and the Cr target during the sputtering deposition process , and by controlling the opening and closing of the baffles in front of the two targets to control the required deposition coating and the deposition time of the Si target and the Cr target on the substrate, in order to obtain the required thickness of the SiN nanolayer and CrSiN nanolayer , where SiN is deposited with a sputtering power of 10W/ cm2 for 2.5min, CrSiN is deposited with a sputtering power of 10W/ cm2 for 5min, and the modulation period is set to Λ=45nm to obtain a SiN/CrSiN nano-multilayer film with a thickness of about 670nm .

实施例2Example 2

选择合金成分为4Cr5MoV1Si,尺寸为600×260×150mm的铝合金压铸模具作为基体,经喷砂、打磨、抛光、清洗、干燥后备用。An aluminum alloy die-casting mold with an alloy composition of 4Cr5MoV1Si and a size of 600×260×150mm was selected as the substrate, and it was sandblasted, polished, polished, cleaned and dried for later use.

将处理好的基体放入超声波清洗机中,按23kHz的频率用丙酮和无水乙醇连续清洗15分钟将清洗后的基体放进多靶磁控溅射镀膜机的真空室内,随后抽真空至9.0×10- 4Pa,然后向其中通入气流量为40sccm的Ar气,此时维持真空室内真空度为3Pa,最后用溅射功率密度为13W/cm2的射频电源对基体进行离子轰击30min,以对基体进行辉光清洗;辉光清洗完成后,开启Cr靶,逐渐调高溅射电流,使Cr靶起辉,将Cr靶的溅射功率密度调至12W/cm2,进行过渡层Cr层的沉积,沉积时间为10min。Put the processed substrate into the ultrasonic cleaning machine, and clean it continuously with acetone and absolute ethanol for 15 minutes according to the frequency of 23kHz. Put the cleaned substrate into the vacuum chamber of the multi-target magnetron sputtering coating machine, and then evacuate to 9.0 ×10 - 4 Pa, and then pass Ar gas with a gas flow rate of 40sccm into it. At this time, the vacuum degree in the vacuum chamber is maintained at 3Pa. Finally, the substrate is bombarded with ions for 30min with a radio frequency power supply with a sputtering power density of 13W/ cm2 . To perform glow cleaning on the substrate; after the glow cleaning is completed, turn on the Cr target, gradually increase the sputtering current to make the Cr target glow, adjust the sputtering power density of the Cr target to 12W/cm 2 , and carry out the transition layer Cr Layer deposition, the deposition time is 10min.

向真空室内通入气流量为40sccm的N2,在Ar-N2的混合气氛中交替打开Si靶和Cr靶的挡板,在溅射沉积过程中不改变Si靶和Cr靶的溅射功率,而通过控制两个靶材前面挡板的开闭来控制所需沉积的涂层以及Si靶和Cr靶在基体上的沉积时间,以此来获得所需厚度的SiN纳米层和CrSiN纳米层,其中SiN以12W/cm2的溅射功率沉淀20min,CrSiN以13W/cm2的溅射功率沉淀40min,设置调制周期为Λ=90nm,得到厚度约为710nm的SiN/CrSiN纳米多层薄膜。Introduce N 2 with a gas flow rate of 40 sccm into the vacuum chamber, open the baffles of the Si target and the Cr target alternately in the Ar-N 2 mixed atmosphere, and do not change the sputtering power of the Si target and the Cr target during the sputtering deposition process , and by controlling the opening and closing of the baffles in front of the two targets to control the required deposition coating and the deposition time of the Si target and the Cr target on the substrate, in order to obtain the required thickness of the SiN nanolayer and CrSiN nanolayer , where SiN was deposited with a sputtering power of 12W/ cm2 for 20min, CrSiN was deposited with a sputtering power of 13W/ cm2 for 40min, and the modulation period was set to Λ=90nm to obtain a SiN/CrSiN nano-multilayer film with a thickness of about 710nm.

实施例3Example 3

选择合金成分为4Cr5MoV1Si,尺寸为600×260×150mm的铝合金压铸模具作为基体,经喷砂、打磨、抛光、清洗、干燥后备用。An aluminum alloy die-casting mold with an alloy composition of 4Cr5MoV1Si and a size of 600×260×150mm was selected as the substrate, and it was sandblasted, polished, polished, cleaned and dried for later use.

将处理好的基体放入超声波清洗机中,按30kHz的频率用丙酮和无水乙醇连续清洗15分钟将清洗后的基体放进多靶磁控溅射镀膜机的真空室内,随后抽真空至9.0×10- 4Pa,然后向其中通入气流量为40sccm的Ar气,此时维持真空室内真空度为3Pa,最后用溅射功率密度为15W/cm2的射频电源对基体进行离子轰击30min,以对基体进行辉光清洗;辉光清洗完成后,开启Cr靶,逐渐调高溅射电流,使Cr靶起辉,将Cr靶的溅射功率密度调至15W/cm2,进行过渡层Cr层的沉积,沉积时间为10min。Put the processed substrate into the ultrasonic cleaning machine, clean it continuously with acetone and absolute ethanol for 15 minutes at a frequency of 30 kHz, put the cleaned substrate into the vacuum chamber of the multi-target magnetron sputtering coating machine, and then vacuumize to 9.0 ×10 - 4 Pa, and then pass Ar gas with a gas flow rate of 40sccm into it. At this time, the vacuum degree in the vacuum chamber is maintained at 3Pa. Finally, the substrate is bombarded with ions for 30min with a radio frequency power supply with a sputtering power density of 15W/ cm2 . To perform glow cleaning on the substrate; after the glow cleaning is completed, turn on the Cr target, gradually increase the sputtering current to make the Cr target glow, adjust the sputtering power density of the Cr target to 15W/cm 2 , and carry out the transition layer Cr Layer deposition, the deposition time is 10min.

向真空室内通入气流量为40sccm的N2,在Ar-N2的混合气氛中交替打开Si靶和Cr靶的挡板,在溅射沉积过程中不改变Si靶和Cr靶的溅射功率,而通过控制两个靶材前面挡板的开闭来控制所需沉积的涂层以及Si靶和Cr靶在基体上的沉积时间,以此来获得所需厚度的SiN纳米层和CrSiN纳米层,其中SiN以15W/cm2的溅射功率沉淀40min,CrSiN以15W/cm2的溅射功率沉淀80min,设置调制周期为Λ=180nm,得到厚度约为750nm的SiN/CrSiN纳米多层薄膜。Introduce N 2 with a gas flow rate of 40 sccm into the vacuum chamber, open the baffles of the Si target and the Cr target alternately in the Ar-N 2 mixed atmosphere, and do not change the sputtering power of the Si target and the Cr target during the sputtering deposition process , and by controlling the opening and closing of the baffles in front of the two targets to control the required deposition coating and the deposition time of the Si target and the Cr target on the substrate, in order to obtain the required thickness of the SiN nanolayer and CrSiN nanolayer , where SiN was deposited with a sputtering power of 15W/ cm2 for 40min, CrSiN was deposited with a sputtering power of 15W/ cm2 for 80min, and the modulation period was set to Λ=180nm to obtain a SiN/CrSiN nano-multilayer film with a thickness of about 750nm.

最后说明的是,以上实施例仅用以说明本发明的技术方案而非限制,尽管参照较佳实施例对本发明进行了详细说明,本领域的普通技术人员应当理解,可以对本发明的技术方案进行修改或者等同替换,而不脱离本发明技术方案的宗旨和范围,其均应涵盖在本发明的权利要求范围当中。Finally, it is noted that the above embodiments are only used to illustrate the technical solutions of the present invention without limitation. Although the present invention has been described in detail with reference to the preferred embodiments, those of ordinary skill in the art should understand that the technical solutions of the present invention can be carried out Modifications or equivalent replacements without departing from the spirit and scope of the technical solution of the present invention shall be covered by the claims of the present invention.

Claims (10)

1.一种高强度复合涂层,其特征在于,包括:1. A high-strength composite coating, characterized in that, comprising: 依次设置的基体、过渡层以及功能层;Substrate, transition layer and functional layer arranged in sequence; 其中所述基体为4Cr5MoV1Si合金,所述过渡层为金属Cr,所述功能层为SiN纳米层和CrSiN纳米层多次交替沉积而成。Wherein the substrate is 4Cr5MoV1Si alloy, the transition layer is metallic Cr, and the functional layer is formed by alternately depositing SiN nano-layers and CrSiN nano-layers multiple times. 2.根据权利要求1所述的一种高强度复合涂层,其特征在于,所述过渡层厚度为150nm~200nm。2. A high-strength composite coating according to claim 1, characterized in that the thickness of the transition layer is 150nm-200nm. 3.根据权利要求1所述的一种高强度复合涂层,其特征在于,所述功能层的厚度为670nm~750nm,其中SiN纳米层与CrSiN纳米层的调制周期比为2:1。3. A high-strength composite coating according to claim 1, characterized in that the thickness of the functional layer is 670nm-750nm, and the modulation period ratio of the SiN nanolayer to the CrSiN nanolayer is 2:1. 4.根据权利要求1所述的一种高强度复合涂层,其特征在于,SiN纳米层和CrSiN纳米层交替沉积的次数为1~15次。4. A high-strength composite coating according to claim 1, characterized in that the number of alternate depositions of SiN nano-layers and CrSiN nano-layers is 1-15 times. 5.一种如权利要求1至4任一项所述的高强度复合涂层的制备方法,其特征在于,包括以下步骤:5. a preparation method of the high-strength composite coating as claimed in any one of claims 1 to 4, is characterized in that, comprises the following steps: (1)对基体进行喷砂、打磨、抛光、清洗以及干燥后备用;(1) Sandblasting, grinding, polishing, cleaning and drying the substrate for subsequent use; (2)将处理完成基体放入超声波清洗机中,在15~30kHZ的频率下使用清洗液进行连续清洗15分钟;(2) Put the processed substrate into an ultrasonic cleaning machine, and use cleaning solution to clean continuously for 15 minutes at a frequency of 15-30kHZ; (3)将清洗后的基体放进多靶磁控溅射镀膜机的真空室内,抽真空至9.0×10-4Pa,然后向其中通入气流量为40sccm的Ar气,此时维持真空室内真空度为3Pa,最后用溅射功率密度为10~15W/cm2的射频电源对基体进行离子轰击30min,以对基体进行辉光清洗;(3) Put the cleaned substrate into the vacuum chamber of a multi-target magnetron sputtering coating machine, evacuate to 9.0×10 -4 Pa, and then pass Ar gas with a gas flow rate of 40 sccm into it, and maintain the vacuum chamber at this time. The degree of vacuum is 3 Pa, and finally, the substrate is bombarded with ions for 30 minutes with a radio frequency power source with a sputtering power density of 10-15W/cm 2 to perform glow cleaning on the substrate; (4)过渡层的制备:开启Cr靶,逐渐调高溅射电流,使Cr靶起辉,将Cr靶的溅射功率密度调至10~15W/cm2,进行过渡层Cr层的沉积,沉积时间为10min;(4) Preparation of the transition layer: turn on the Cr target, gradually increase the sputtering current to make the Cr target glow, adjust the sputtering power density of the Cr target to 10-15W/cm 2 , and deposit the Cr layer of the transition layer. Deposition time is 10min; (5)功能层的制备:向真空室内通入流量为40sccm的N2,在Ar-N2的混合环境下,交替地开启Si靶材与Cr靶材前面的挡板,溅射沉积纳米级的多层膜,该多层膜是由多个SiN纳米层和CrSiN纳米层交替堆叠而成,同时调节Si靶材和Cr靶材的溅射功率密度和沉积时间,以控制SiN纳米层和CrSiN纳米层的调制周期。(5) Preparation of the functional layer: N 2 with a flow rate of 40 sccm is passed into the vacuum chamber, and in the mixed environment of Ar-N 2 , the baffles in front of the Si target and the Cr target are alternately opened, and the nano-scale The multilayer film is composed of multiple SiN nanolayers and CrSiN nanolayers stacked alternately, and the sputtering power density and deposition time of the Si target and the Cr target are adjusted at the same time to control the SiN nanolayer and CrSiN Modulation period of the nanolayer. 6.根据权利要求5所述的一种高强度复合涂层的制备方法,其特征在于,步骤(2)中的清洗液包括丙酮和无水乙醇。6. the preparation method of a kind of high-strength composite coating according to claim 5 is characterized in that, the cleaning solution in step (2) comprises acetone and dehydrated alcohol. 7.根据权利要求5所述的一种高强度复合涂层的制备方法,其特征在于,步骤(5)中SiN纳米层和CrSiN纳米层的溅射功率密度均为10~15W/cm2。7 . The method for preparing a high-strength composite coating according to claim 5 , wherein the sputtering power densities of the SiN nano-layer and the CrSiN nano-layer in step (5) are both 10-15 W/cm 2 . 8.根据权利要求5所述的一种高强度复合涂层的制备方法,其特征在于,步骤(5)中SiN纳米层的沉积时间为2.5~40min。8 . The method for preparing a high-strength composite coating according to claim 5 , wherein the deposition time of the SiN nano-layer in step (5) is 2.5 to 40 minutes. 9.根据权利要求5所述的一种高强度复合涂层的制备方法,其特征在于,步骤(5)中CrSiN纳米层的沉积时间为5~80min。9. The method for preparing a high-strength composite coating according to claim 5, characterized in that the deposition time of the CrSiN nano-layer in step (5) is 5-80 min. 10.一种如权利要求1至4任一项所述的高强度复合涂层在铝合金压铸模具上的应用。10. An application of the high-strength composite coating according to any one of claims 1 to 4 on an aluminum alloy die-casting mold.
CN202310483332.9A 2023-04-28 2023-04-28 High-strength composite coating, preparation method and application thereof Pending CN116445857A (en)