CN120356830B - Preparation method of multi-chip connecting structure - Google Patents
Preparation method of multi-chip connecting structureInfo
- Publication number
- CN120356830B CN120356830B CN202510779783.6A CN202510779783A CN120356830B CN 120356830 B CN120356830 B CN 120356830B CN 202510779783 A CN202510779783 A CN 202510779783A CN 120356830 B CN120356830 B CN 120356830B
- Authority
- CN
- China
- Prior art keywords
- layer
- copper
- chip
- bonding
- rdl
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Abstract
The invention belongs to the technical field of chips, and particularly relates to a preparation method of a multi-chip connection structure. The method comprises the steps of coating a release layer and an adhesive layer on a substrate, coating copper column bumps on a chip, temporarily bonding the chip on the adhesive layer, embedding the copper column bumps on a control part into the adhesive layer, forming a plastic layer on the adhesive layer, wrapping the chip and the residual copper column bumps by the plastic layer, forming a first module by the chip and the plastic layer together, stripping the adhesive layer, exposing the copper column bumps embedded into the adhesive layer, depositing a nonmetallic medium material on the surface of the first module with the copper column bumps to modify the copper column bumps, not exposing the two sides of the copper column bumps, carrying out copper-copper bonding on the residual exposed surface of the copper column bumps and a TSV intermediate layer, removing the redundant silicon substrate of the TSV intermediate layer, forming a complete RDL layer at the bottom of the second module, and manufacturing bumps on the surface of the complete RDL layer. The invention improves the welding reliability, signal integrity and heat dissipation performance of the multi-chip connecting structure.
Description
Technical Field
The invention belongs to the technical field of chips, and particularly relates to a preparation method of a multi-chip connection structure.
Background
Conventionally, uPad (micro bumps), such as micro bumps made of Cu/Ni/Au alloy solder or Cu/Ni/SnAg alloy solder, are typically electroplated on a TSV interposer, and then a chip is soldered on the TSV interposer by Flip chip, and then the chip is encapsulated.
The technical problems of the preparation are as follows:
The reliability of welding, namely the reliability problem of the micro-convex points is increasingly outstanding, and the defects of cold joint, crack and the like are easy to occur, so that the long-term stability of the chip is affected.
Signal integrity-as the frequency of the signal increases, the parasitic capacitance and inductance of the micro-bumps and solder can affect the signal integrity, limiting the data transmission rate.
And the thermal management is that the thermal resistance of the micro-convex points and the solder is higher, so that the heat dissipation performance of the chip can be influenced.
Disclosure of Invention
Aiming at the defects of the prior art, the invention aims to provide a preparation method of a multi-chip connecting structure.
To achieve the above and other related objects, the present invention provides the following technical solutions:
The preparation method of the multi-chip connecting structure comprises the following steps:
coating a release layer on the substrate, and coating an adhesive layer on the release layer;
The chip comprises an SOC Die and an HBM Die, copper stud bumps are arranged on the chip, the chip is temporarily bonded on the adhesive layer, and the copper stud bumps of the control part are embedded into the adhesive layer;
Forming a plastic sealing layer on the bonding layer, wherein the plastic sealing layer wraps the chip and the copper stud bumps of the rest part, and the chip and the plastic sealing layer form a first module together;
stripping the bonding layer, exposing the copper stud bump embedded in the bonding layer, depositing a nonmetallic dielectric material on the surface of the module with the copper stud bump to modify the copper stud bump, so that two sides of the copper stud bump are not exposed any more, and carrying out copper-copper bonding (Cu-Cu bonding) on the residual exposed surface of the copper stud bump and the TSV interposer;
And removing the redundant silicon substrate of the TSV medium layer to obtain a second module, constructing a complete RDL layer at the bottom of the second module, and manufacturing a bump on the surface of the complete RDL layer.
In the above technical scheme, 1) during plastic packaging, the plastic packaging layer only wraps a part of the copper stud bumps of the chip, and the rest is embedded into the adhesive layer. Therefore, the plastic layer can protect the cylindrical surface of the copper stud bump, avoid being corroded by water vapor and avoid metal migration. 2) After the bonding layer is stripped, a nonmetallic dielectric material is deposited to modify the copper stud bump, so that the cylindrical surface of the copper stud bump can be protected. 3) Copper-copper bonding is performed on the remaining exposed surfaces of the copper stud bumps and the TSV interposer, which can also be considered as forming copper-copper bonds for module one and module two.
Compared with the micro-bump welding mode used in the traditional CoWoS-S technology, the copper-copper bonding technology adopted by the invention avoids the problems of uneven heating, concave or convex weldment and the like caused by solder or solder paste reflow welding, and improves the flatness and the electrical connection reliability of a bonding interface. The preparation method of the invention improves welding reliability, signal integrity and heat dissipation performance.
In one embodiment, the temporary bonding step comprises the steps of symmetrically arranging every two HBM Die on two sides of one SOC Die by using a bonding machine, bonding the copper stud bumps of the HBM Die and the SOC Die face downwards with the bonding layer, and controlling the depth of embedding the copper stud bumps into the bonding layer to be 2-3 mu m, wherein the total number of the HBM Die is more than or equal to 2, and the total number of the SOC Die is more than or equal to 1.
In one embodiment, the metal pad of the SOC Die has copper stud bumps with a height of 4-8 μm and a width of 5-25 μm, and the metal pad of the HBM Die has copper stud bumps with a height of 4-8 μm and a width of 5-25 μm.
In one embodiment, the method for preparing the TSV interposer includes the steps of:
Using an anisotropic etching process to manufacture transverse and longitudinal deep holes on a silicon substrate, wherein the longitudinal deep holes are connected through the transverse deep holes;
Depositing an insulating layer in a deep hole of a silicon substrate, depositing a blocking layer on the insulating layer, depositing or not depositing a seed layer, electroplating and filling a metal material in the deep hole to remove redundant metal materials on the surface of the silicon substrate, then depositing an insulating material on the surface of the silicon substrate by using an RDL process, specifically, coating photoresist on the insulating material, exposing, developing to form an RDL circuit pattern, sputtering and depositing and/or electroplating metallic copper in the RDL circuit pattern to form an interconnection line, forming an intermediate connecting layer, stripping the photoresist, and obtaining the TSV intermediate layer.
Further, when the deep hole is electroplated with a metal material, the metal material comprises copper, and when the remaining exposed surface of the copper stud bump is subjected to copper-copper bonding with the TSV interposer, the exposed surface is subjected to copper-copper bonding with the intermediate connection layer.
In one embodiment, removing the excess silicon substrate of the TSV interposer includes the steps of:
and (3) thinning the thickness d1 of the redundant silicon substrate to 3-10 mu m by using a grinder, etching the bottom of the silicon substrate by using an etching process to expose a part of deep holes wrapped by the silicon substrate, wherein the exposed thickness of the deep holes is 1-5 mu m, depositing nonmetallic dielectric materials on two sides of the exposed deep holes by using a PECVD process, and flattening the bottom of the silicon substrate by using a CMP process.
Optionally, the non-metallic dielectric material includes at least one of silicon nitride and silicon dioxide.
In one embodiment, building a complete RDL layer on the bottom of module two includes the steps of:
forming a passivation layer at the bottom of the second module, covering the passivation layer by using a mask, exposing, dissolving the passivation layer outside the mask, leaving a designed pattern on the second module, sputtering a titanium layer and a copper layer on the designed pattern to form a PVD layer, and forming a first RDL layer by the PVD layer and the rest passivation layer;
Forming a photoresist layer on the first RDL layer, covering the photoresist layer by using a mask, exposing, dissolving the photoresist layer outside the mask, leaving a designed pattern on the first RDL layer, and electroplating copper on the designed pattern to form a conductive circuit;
Removing the residual photoresist, reserving conductive lines formed by electroplating, etching to remove unnecessary conductive lines, reserving only conductive lines connected with the PVD layer, generating a vacant gap after etching, forming a protective layer in the gap, and forming a second RDL layer by the conductive lines and the protective layer;
the first RDL layer and the second RDL layer together form a complete RDL layer.
In one embodiment, the parameters of temporary bonding comprise initial contact pressure of 0.5-1.0MPa, copper stud bumps in contact with the bonding layer but not embedded, embedding stage pressure of 2.5-3.5MPa, and pressure maintaining time of 8-15 seconds.
In one embodiment, the molding compound is used for molding, and the preparation of the molding compound comprises the following steps:
bisphenol F type epoxy resin and reactive diluent are uniformly mixed to obtain resin mixed solution,
Uniformly mixing large-size silicon dioxide, small-size silicon dioxide and nano particles to obtain mixed powder;
slowly adding the resin mixed solution into the mixed powder, and stirring to obtain a mixture;
adding an antifoaming agent and a leveling agent into the mixture, and stirring to obtain a mixed solution;
slowly adding the curing agent into the mixed solution, stirring, and vacuum defoaming to obtain a molding compound;
Wherein the particle size of the large-size silica is 10-20 μm, the particle size of the small-size silica is 0.1-0.5 μm, and the reactive diluent comprises siloxane oligomer.
Further, the addition amount of the large-size silica is 50-70 parts by weight, the addition amount of the small-size silica is 10-15 parts by weight, and the addition amount of the nano particles is 1-10 parts by weight.
Alternatively, the particle size of the nanoparticle is 50-100nm. The nanoparticles comprise alpha phase nano silicon nitride particles.
The beneficial effects of the invention are as follows:
Compared with the traditional micro-bump welding, the structure of the invention has higher transmission rate, and the Cu-Cu bonding has lower resistance and inductance, so that higher data transmission rate can be realized.
The structure of the invention has higher I/O density, and Cu-Cu bonding can realize smaller bonding spacing, thereby supporting higher I/O density.
The structure of the invention has better reliability that Cu-Cu bonding has higher bonding strength and better thermal cycle performance, and the long-term reliability of the chip is improved.
The structure of the invention has better thermal performance, cu-Cu bonding has lower thermal resistance, and is beneficial to heat dissipation of chips.
Specifically, the exposed surface of the chip copper pillar bump is directly bonded with the intermediate connection layer of the TSV intermediate layer, and the TSV intermediate layer does not need to additionally manufacture copper pillars or micro bumps, so that the process flow is simplified, the manufacturing cost is reduced, and meanwhile, the bonding precision and the interconnection density are improved.
Further, in the plastic packaging step, the exposed copper stud bumps are wrapped by the molding compound, so that the molding compound is used as a protective material for preventing copper metal migration, and the side surfaces of the copper stud bumps are protected from oxidization, so that the long-term reliability of the packaging structure is further enhanced.
After stripping the bonding layer, depositing silicon nitride and silicon dioxide on the exposed surface of the copper stud bump, and forming three-layer protection structures (plastic sealing layers, silicon nitride and silicon dioxide) on two sides of the copper stud bump, so that the side surface of the copper stud bump is effectively protected, oxidation and metal migration are prevented, and meanwhile, the exposed surface of the copper stud bump is reserved, and subsequent bonding is facilitated.
In the RDL process, through multilayer rerouting (a first RDL layer and a second RDL layer), efficient reconstruction and distribution of the circuit are realized, and flexibility and integration density of signal transmission are remarkably improved.
Furthermore, in the process of preparing the first module, the invention also provides chip bonding parameters, ensures that the depth of the copper stud bump embedded into the bonding layer is accurately controlled to be 2-3 mu m, avoids offset or uneven embedding of the copper stud bump caused by instantaneous high pressure, and improves the position stability and the structural reliability of the chip in the plastic packaging process.
The invention also provides a molding compound formula, and the quality of the plastic sealing layer is further improved. The molding compound adopts bisphenol F epoxy resin with low viscosity and high reactivity, and combines with reactive diluent (siloxane oligomer), thereby reducing the viscosity of the resin system, improving the fluidity, effectively filling small gaps and reducing bubble generation. The efficient defoaming agent and the leveling agent are added, the defoaming agent can quickly eliminate bubbles in the mixing and encapsulating process, the leveling agent can improve fluidity and reduce surface defects, so that no bubble defects exist in the plastic sealing layer, and the mechanical strength and the electrical performance of the packaging structure are improved. The multi-stage composite filler (large-size silica, small-size silica and nano silicon nitride particles) is adopted, so that the packing density of the filler is optimized, the thermal expansion coefficient is reduced, the toughness and the shock resistance of the molding compound are enhanced, and the reliability of the packaging structure is further improved.
Drawings
In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings that are needed for the description of the embodiments will be briefly described below, and it is obvious that the drawings in the following description are only some embodiments of the present invention, and that other drawings may be obtained according to these drawings without inventive effort for a person skilled in the art.
FIG. 1 is a schematic diagram of a step of preparing a module according to embodiment 1 of the present invention;
FIG. 2 is a schematic diagram showing a process for preparing a module according to embodiment 1 of the present invention;
FIG. 3 is a schematic diagram showing a process for preparing a module according to embodiment 1 of the present invention;
FIG. 4 is a schematic diagram showing the structure of the peeling step in embodiment 1 of the present invention;
FIG. 5 is a schematic diagram of a hybrid bonding step in embodiment 1 of the present invention;
FIG. 6 is a schematic diagram of a bonding via exposure process step in embodiment 1 of the present invention;
FIG. 7 is a schematic diagram of the RDL process step in embodiment 1 of the present invention;
FIG. 8 is a schematic diagram of the RDL process step in embodiment 1 of the present invention;
FIG. 9 is a schematic diagram of a bump process step in embodiment 1 of the present invention;
The circuit board is characterized by comprising a substrate 1, a release layer 2, an adhesive layer 3, a 4.SOC Die;5.HBM Die;6, a plastic sealing layer 7, a first module 8, an exposed surface 9, a TSV intermediate layer 10, a deep hole 11, an intermediate connection layer 12, a second module 13, a PVD layer 14, a first RDL layer 15, an electric conduction line 16, a second RDL layer 17, a complete RDL layer 18 and a bump.
Fig. 1-9 together form a flow chart for preparing a multi-chip connection structure.
Detailed Description
The following describes the preparation method of the multi-chip connection structure according to the present invention in further detail with reference to the accompanying drawings and specific examples. Advantages and features of the invention will become more apparent from the following description and from the claims. It should be noted that the drawings are in a very simplified form and are all to a non-precise scale, merely for convenience and clarity in aiding in the description of embodiments of the invention.
In the description of the present invention, unless explicitly specified and limited otherwise, the terms "connected," "connected," and "connected" are to be construed broadly, and may be, for example, fixedly connected, detachably connected, integrally connected, mechanically connected, electrically connected, directly connected, indirectly connected through an intermediate medium, and in communication with each other between two elements, and may be wireless or wired. The specific meaning of the above terms in the present invention will be understood in specific cases by those of ordinary skill in the art.
Unless otherwise specified, the materials used in the examples are readily available from commercial companies.
The SOC (System on Chip) Die and HBM (High Bandwidth Memory ) Die are named directly in english without repeating chinese comments, and the chips (SOC Die and HBM Die) used in the present invention are commercially available conventionally, and the specific mechanism thereof is also known to those skilled in the art and will not be repeated.
The preparation method of the multi-chip connection structure, referring to fig. 1-9, specifically comprises the following steps:
1. preparation module one:
Referring to fig. 1, a glass substrate is selected as a base material 1, a release material layer is coated on the base material 1 to form a release layer2, and an adhesive material layer is coated on the release layer2 to form an adhesive layer 3. Wherein the release material includes, but is not limited to, photosensitive material, heat release tape. The adhesive material includes, but is not limited to, a die temporary adhesive material, a temporary adhesive film.
Selecting a chip, wherein the chip is provided with an SOC Die 4 and an HBM Die 5, a copper column bump is arranged on a metal pad of the SOC Die 4, the height of the copper column bump is 4-8 mu m, and the width of the copper column bump is 5-25 mu m. The copper stud bump of SOC Die 4 is electrically connected to the wiring within SOC Die 4.
The metal pad of HBM Die 5 is also provided with copper stud bumps, the height of the copper stud bumps is 4-8 μm, and the width of the copper stud bumps is 5-25 μm. To ensure high production process yields, HBM Die 5 needs to maintain consistent height and width with SOC Die 4. The copper stud bump of HBM Die 5 is electrically connected to the wiring within HBM Die 5.
Chip bonding (Die bond) referring to fig. 2, HBM Die 5 and SOC Die 4 are temporarily bonded on adhesive layer 3 using a chip bonding process. The specific number and layout can be that a bonding machine is used for symmetrically arranging every two HBM Die 5 on two sides of one SOC Die 4, copper column bumps of the HBM Die 5 and the SOC Die 4 are bonded with the bonding layer 3 downwards, and the depth of the copper column bumps embedded into the bonding layer 3 is controlled to be 2-3 mu m, so that subsequent plastic packaging is facilitated. Wherein the total number of HBM Die 5 is more than or equal to 2, and the total number of SOC Die 4 is more than or equal to 1.
And (3) plastic packaging, namely, referring to fig. 3, using a molding compound to plastic package the HBM Die 5 and the SOC Die 4, forming a plastic packaging layer 6 on the adhesive layer 3, wherein the plastic packaging layer 6 contains the HBM Die 5 and the SOC Die 4, and the HBM Die 5, the SOC Die 4 and the plastic packaging layer 6 together form a module I7. During plastic packaging, the molding compound also wraps the copper stud bump exposed outside and not embedded with the bonding layer 3, and the effect is that the molding compound can be used as a protection material of the copper stud bump, so that copper metal migration is avoided, the side face of the copper stud bump can be protected, and oxidization is prevented.
Grinding (milling) this step is an optional step. The surface of the plastic sealing layer 6 is ground and flattened by a grinding process by using a precise grinding machine.
2. Peeling-off referring to fig. 4, the adhesive layer 3 is peeled off, the adhesive layer 3 connected to the first module 7 is removed by a debonding process (Debond), and the debonding is performed according to the instruction of the adhesive material by using the characteristics of the adhesive material such as thermal slip removal or laser deagglomeration or solvent-assisted peeling. After removal of the adhesive layer 3, the corresponding release layer 2 and substrate 1 are also removed. After the bonding layer 3 is de-bonded, the surface of the first module 7 is cleaned, residues of the de-bonding process are removed, and the cleaning and drying are carried out.
After the adhesive layer 3 is stripped, copper stud bumps embedded in the adhesive layer 3 in the early stage are exposed to the outside, so that the copper stud bumps of the chip are partially arranged in the plastic sealing layer 6 and partially arranged outside the plastic sealing layer 6.
3. Copper stud bump of modified chip referring to fig. 4, a non-metal dielectric material is deposited on the side of the module 7 with copper stud bump to modify copper stud bump, silicon nitride (SiNx) is deposited on the bottom of the molding layer 6, i.e. the side with copper stud bump, with a deposition thickness of 250-2000 a, silicon dioxide is deposited on silicon nitride (SiO 2),SiO2 with a deposition thickness of 5000-30000 a), and then the thickness of SiO 2 is ground to 3000-18000 a with CMP (chemical mechanical polishing) technique, wherein 1 a=1×10 (-10) m.
After that, the two sides of the copper stud bump of the chip are not exposed any more, and the two sides of the copper stud bump of the chip have a three-layer structure, wherein the first layer is a plastic layer 6, the second layer is silicon nitride, and the third layer is SiO 2 from top to bottom. Silicon nitride and SiO 2 are not shown in fig. 4.
The bottom of the copper stud bump is uncovered and exposed, and for ease of illustration, is designated herein as exposed surface 8, the exposed surface 8 being configured to facilitate subsequent bonding.
4. Hybrid bond (Hybrid bond) referring to fig. 5, a module 7 and a TSV interposer (TSV interposer) 9 are connected, specifically, the TSV interposer 9 is taken out, and the TSV interposer 9 is prepared by manufacturing transverse and longitudinal deep holes 10 on a silicon substrate by using a dry etching process, that is, an anisotropic etching process, and the longitudinal deep holes 10 are connected through the transverse deep holes 10. In order to precisely etch the deep hole 10, the unnecessary side walls are prevented from being etched, and the side walls can be etched and passivated, namely, a section of deep hole 10 is etched on a silicon substrate by using plasma, then a layer of thin insulating material such as silicon dioxide is deposited on the side walls of the deep hole 10 by using passivation gas (such as silane gas) to form a passivation layer, and then the plasma is switched to continuously etch the next section of deep hole 10 in a specific direction. This also maintains a sufficient etched hole diameter and depth.
To ensure that passivation layers are formed in the recesses 10, a thin layer of insulating material, such as silicon dioxide, is deposited in the recesses 10 of the silicon substrate after etching to form an insulating layer, ti (titanium) or TiN (titanium nitride) is deposited on the insulating layer as a barrier layer, and then a filler metal material, which is copper, is electroplated in the recesses 10. If other metal materials are selected, a further layer of copper can be deposited as a seed layer on the barrier layer, and the filler metal material can be electroplated.
And then depositing insulating materials on the surface of the silicon substrate by utilizing an RDL (Redistribution Layer ) process, wherein the insulating materials comprise silicon nitride (SiNx), silicon dioxide and NDC (silicon carbide film). Then, photoresist is coated on the insulating material, exposure and development are carried out by a photoetching machine to form an RDL circuit pattern, metal copper is sputtered and deposited and/or electroplated in the RDL circuit pattern, so that interconnection lines are manufactured, an intermediate connection layer 11 is formed, and the intermediate connection layer 11 is electrically connected with the metal material in the deep holes 10. The photoresist is subsequently stripped and the excess residue is cleaned. Through the foregoing steps, the TSV interposer 9 is prepared.
The exposed surface 8 of the chip copper stud bump is then connected to the intermediate connection layer 11 in a Cu-Cu bond (copper-copper bond). Copper-copper bonding belongs to metal-metal bonding, and copper-copper bonding is realized by mutual diffusion of copper atoms under certain bonding process conditions. Specifically, the exposed surfaces 8 of the copper stud bumps of the HBM Die 5 and the SOC Die 4 are aligned with the intermediate connection layer 11 of the TSV interposer 9 by using a bonder, and the copper stud bumps are interconnected with the intermediate connection layer 11 by thermocompression bonding or low temperature bonding. If hot-press bonding is selected, the bonding parameters are 250-400 ℃ under the protection of nitrogen, 5-50MPa and 5-30 minutes. Copper atoms diffuse at high temperature and high pressure to form intermetallic eutectic connections. If low-temperature bonding is selected, firstly, formic acid vapor or formic acid solution is used for pretreatment of the surface to be bonded, the surface roughness is increased, the bonding temperature is reduced, then bonding is carried out, and the bonding parameters are 150-250 ℃, 10-20MPa and 10-60 minutes.
In the prior art, in CoWoS-S (chip on substrate wafer with silicon interposer), a micro bump (uBump) soldering method is generally used, and solder or solder paste is used to reflow-solder the chip and TSV interposer 9, so that the problems of uneven heating, concave solder part, and concave depression are easily occurred. Unlike the prior art, the invention does not additionally manufacture copper pillars and micro bumps on the TSV interposer 9. The invention realizes copper-copper bonding by utilizing the copper stud bumps of the intermediate connecting layer 11 made of copper, the HBM Die 5 and the SOC Die 4.
5. The bonding via exposure process (BVR) VIA REVEAL refers to fig. 5 and 6, in which the bottom of the TSV interposer 9 is subjected to grinding, dry etching process, PECVD (plasma enhanced chemical vapor deposition), CMP (chemical mechanical polishing), through which the redundant silicon substrate at the bottom of the TSV interposer 9 can be ground off, and if all the redundant silicon substrate is directly removed by the grinding process, a plurality of problems, such as 1) cracking and chipping, are likely to occur, and 1) local stress is likely to be introduced in the brittle silicon material as a mechanical process, resulting in micro cracks or edge chipping, reducing structural integrity and long-term reliability. 2) Lattice damage, namely grinding can damage the lattice structure of the silicon surface to form a defect layer, influence carrier mobility, increase leakage current and reduce device performance. 3) Uneven thickness, grinding is difficult to accurately control the removal amount of the silicon substrate, and can lead to inconsistent TSV heights, and influence the alignment and interconnection quality of three-dimensional integration.
The lateral and longitudinal deep holes 10 of the present application constructed in the previous step are complicated in structure, do not avoid the above problems, and cannot directly remove all the unnecessary silicon substrate using a single grinding process.
The excess silicon substrate is thus removed here by a combination of processes, in particular:
The bottom of the silicon substrate, i.e., the side not contacting the first module 7, is ground using a grinder, and the bottom thickness d1 of the silicon substrate is thinned to 3-10 μm, where d1 is the thickness from the deep hole 10 to the bottom surface of the silicon substrate. And then etching the bottom of the silicon substrate by a dry etching process to expose a part of deep holes 10 wrapped by the silicon substrate, wherein the thickness of the exposed deep holes 10 is 1-5 mu m. The purpose of this is to expose the copper electroplated in the recess 10.
Silicon nitride (SiNx) is then deposited on both sides of the exposed recess 10 using a PECVD (plasma enhanced chemical vapor deposition) process, and silicon dioxide is deposited on the silicon nitride, so that the electroplated copper within the recess 10 is protected from being exposed on both sides.
The bottom of the silicon substrate is then planarized using CMP (chemical mechanical polishing) to remove excess copper and silicon dioxide.
Through the above steps, all the redundant silicon substrate is removed, and the TSV interposer 9 with a proper thickness is prepared, which is named as a second module 12 for convenience of description.
Rdl (Redistribution Layer, re-wiring layer) process:
referring to fig. 7 and 8, the RDL process is used to reroute the bottom of the second module 12, specifically:
the glue is applied by coating Polyimide (PI) on the bottom of the second module 12 as a passivation layer to provide electrical insulation and mechanical protection.
And exposing, namely covering the passivation layer by using a mask plate, exposing, and transferring the designed pattern on the mask plate to the passivation layer by using illumination.
Developing by dissolving the passivation layer outside the reticle with a developer, thus leaving a designed pattern on the second module 12. Wherein the developer comprises TMAH (tetramethylammonium hydroxide) or other developer.
Physical Vapor Deposition (PVD), in which a layer of titanium (Ti) and copper (Cu) is sputtered onto the developed surface in a designed pattern to form a PVD layer 13. Wherein titanium is used as an adhesion layer to prevent copper diffusion, and copper is used as an electroplating seed layer. Thus, the PVD layer 13 and the remaining passivation layer constitute a first RDL layer 14. The PVD layer 13 is electrically connected to the deep holes 10. This results in the structure of fig. 7.
The foregoing steps are then repeated:
photoresist is spin-coated on the surface of the first RDL layer 14 to form a photoresist layer.
And (3) secondary exposure, namely covering the photoresist layer by using a mask plate, exposing, and transferring the designed pattern on the mask plate onto the photoresist layer by using illumination.
And secondary developing by dissolving the photoresist layer outside the reticle with a developer, thus leaving a designed pattern on the first RDL layer 14. Wherein the developer comprises TMAH (tetramethylammonium hydroxide) or other developer.
Electroplating, namely electroplating copper on the surface after secondary development, and forming a conductive circuit 15 on the designed pattern.
Photoresist stripping, namely removing redundant photoresist by using chemical stripping liquid, and reserving the conductive circuit 15 formed by electroplating.
Etching, namely etching to remove unnecessary wire lines 15, only reserving the conductive lines 15 connected with the PVD layer 13, generating empty gaps after etching, filling or coating protective materials in the gaps to form a protective layer, wherein the protective materials can be Polyimide (PI), so that the reliability of the whole structure is ensured.
The conductive trace 15 and the protective layer thus formed by electroplating constitute a second RDL layer 16.
The first RDL layer 14 and the second RDL layer 16 together form a complete RDL layer 17 to enable the reconfiguration and distribution of the lines. This results in the structure of fig. 8.
7. Bump process referring to fig. 9, a bump 18 is fabricated on the surface of the complete RDL layer 17 using a C4 bump process, and the bump 18 needs to be electrically connected to the complete RDL layer 17, i.e., the bump 18 is electrically connected to the conductive circuit 15, so as to achieve circuit connection.
Example 1 in the step of molding the first module 7, the molding compound also covered the copper stud bumps exposed without the embedded adhesive layer 3.
To achieve such a structure, it is necessary to control the depth of the chip embedded adhesive layer 3, and example 1 shows that the depth of the copper stud bump embedded adhesive layer 3 is controlled to be 2-3 μm, which is convenient for the subsequent plastic packaging.
But it is also necessary to control the parameters of chip bonding, and the parameters of the material and the plastic package of the selected molding compound, so as to ensure that no air bubbles are generated in the plastic package layer 6 and the chip is not shifted by impact.
Accordingly, these parameters are provided in the following examples.
Example 2
In this embodiment, specific parameters of die bonding are provided:
And (3) step control of bonding pressure:
the initial contact pressure is 0.5-1.0MPa, so that the copper stud bump is ensured to be in contact with the bonding layer 3 but not embedded;
the pressure of the embedding stage is 2.5-3.5MPa, and the depth of the copper pillar bump embedded into the bonding layer 3 is controlled to be 2-3 mu m;
dwell time is 8-15 seconds, avoiding excessive deformation of the adhesive layer 3.
The remainder was the same as in example 1.
The classification pressure can avoid offset or uneven embedding of the copper stud bump caused by instantaneous high pressure.
Example 3
In this example, a specific molding compound is provided, and the preparation of the molding compound comprises the following steps in parts by weight:
22 parts of bisphenol F type epoxy resin and 6 parts of reactive diluent are taken and put into a container, and are magnetically stirred for 15-20 minutes at the room temperature of 300-500rpm, and uniformly mixed to obtain a resin mixed solution.
Taking 50 parts of large-size silicon dioxide with the particle size of 10-20 mu m, 10 parts of small-size silicon dioxide with the particle size of 0.1-0.5 mu m and 2 parts of nano particles with the particle size of 50-100nm, adding the three powder into a high-speed mixer, dry-mixing for 5-10 minutes, and uniformly mixing to obtain mixed powder.
Slowly adding the resin mixed solution into the mixed powder, stirring while adding, dispersing at 1000-1500rpm for 10-15 min, gradually increasing the rotation speed to 2000-2500rpm, and continuing dispersing for 15-20 min to obtain the mixture.
To the mixture, 0.3 part of an antifoaming agent and 0.2 part of a leveling agent were sequentially added, and stirring was continued at a speed of 1500rpm for 5 minutes to obtain a mixed solution. Wherein the defoamer reduces air bubbles in the molding compound. The leveling agent can improve the fluidity of the molding compound.
Before the use, 9.5 parts of modified amine curing agent is slowly added into the mixed solution, stirred for 10 minutes at 1000rpm, and then defoamed in vacuum, namely, the mixture is stirred and defoamed for 15 minutes at a speed of 800rpm under the condition that the vacuum degree is minus 0.095MPa, and bubbles in the mixture are removed, so that the molding compound is obtained.
Among the above, the specific selection of the raw materials used in this example is:
Bisphenol F epoxy resin with epoxy equivalent weight of 160-180g/eq and viscosity of 3000-4000cps (25 ℃), and NPEF-170 bisphenol F epoxy resin can be selected;
Reactive diluent, namely siloxane oligomer Evonik TEGOPREN 6875;
Large-size silicon dioxide, namely spherical, ADMAFINE ℃ SO-E5 and Admatechs;
The small-size silicon dioxide is spherical, and the Admatechs is SO-C3;
the nanometer particles are alpha-phase nanometer silicon nitride particles (Si 3N4), the grain diameter is 50-100nm, and the silicon content is 99%;
defoaming agent BYK-A530, pick;
leveling agent BYK-354, pick;
modified amine curing agent, huntsman Aradur 2958.
Further, it is worth noting that the present invention,
(1) Resin system:
The main resin is bisphenol F type epoxy resin with low viscosity and high reactivity. Compared with the traditional bisphenol A epoxy resin, the selected bisphenol F resin has lower viscosity, better fluidity and faster curing speed, and is beneficial to filling fine gaps and reducing bubble generation.
Reactive diluents-small amounts of siloxane oligomers with epoxide functions are added. The selected siloxane oligomer not only can reduce the viscosity of a resin system and improve the fluidity, but also can react with epoxy resin to form a siloxane chain segment with certain flexibility, so that the toughness and the shock resistance of the molding compound are improved.
(2) The multi-stage composite filler is prepared by combining fillers with different sizes and functions, wherein the large-size silica is used as main filler, the particle size is 10-20 mu m, and the weight parts are 50-70 parts. Providing a low coefficient of thermal expansion and a high loading. The small-size silicon dioxide is submicron spherical silicon dioxide, the particle size is 0.1-0.5 mu m, and the weight parts are 10-15 parts. Filling gaps among large particles, improving bulk density and reducing viscosity. The nano particles are alpha-phase nano silicon nitride (Si 3N4) particles, are dispersed in the matrix, have high surface activity, and form strong chemical bonding with the matrix, so that the interface strength is improved.
(3) The additive is an efficient organic silicon defoamer, and bubbles generated in the mixing and encapsulating process can be rapidly eliminated. The leveling agent is selected from acrylic ester leveling agents which can improve fluidity and reduce surface defects.
(4) And (3) the curing agent is a modified amine curing agent with low viscosity and high reactivity. The curing agent can be cured rapidly at a lower temperature, and shrinkage and stress in the curing process are reduced.
(5) The cured molding compound forms a multiphase composite structure:
continuous phase, polymer network formed by crosslinking epoxy resin and reactive diluent and curing agent.
Dispersed phase large-size spherical silica particles are uniformly distributed in the matrix. The small-sized silica fills in the gaps between the large particles. The core-shell nanoparticles are dispersed in the matrix and form strong chemical bonds with the matrix.
It is apparent that the above examples are given by way of illustration only and are not limiting of the embodiments. Other variations or modifications of the above teachings will be apparent to those of ordinary skill in the art. It is not necessary here nor is it exhaustive of all embodiments. While still being apparent from variations or modifications that may be made by those skilled in the art are within the scope of the invention.
Claims (9)
1. The preparation method of the multi-chip connecting structure is characterized by comprising the following steps:
coating a release layer on the substrate, and coating an adhesive layer on the release layer;
The chip comprises an SOC Die and an HBM Die, copper stud bumps are arranged on the chip, the chip is temporarily bonded on the adhesive layer, and the copper stud bumps of the control part are embedded into the adhesive layer;
Forming a plastic sealing layer on the bonding layer, wherein the plastic sealing layer wraps the chip and the copper stud bumps of the rest part, and the chip and the plastic sealing layer form a first module together;
Stripping the bonding layer, exposing the copper stud bump embedded in the bonding layer, depositing a nonmetallic dielectric material on the surface of the module with the copper stud bump to modify the copper stud bump, so that two sides of the copper stud bump are not exposed any more, and carrying out copper-copper bonding on the residual exposed surface of the copper stud bump and the TSV interposer;
Removing the redundant silicon substrate of the TSV medium layer to obtain a second module, constructing a complete RDL layer at the bottom of the second module, and manufacturing a bump on the surface of the complete RDL layer;
the preparation method of the TSV medium layer comprises the following steps:
Using an anisotropic etching process to manufacture transverse and longitudinal deep holes on a silicon substrate, wherein the longitudinal deep holes are connected through the transverse deep holes;
Depositing an insulating layer in a deep hole of a silicon substrate, depositing a blocking layer on the insulating layer, depositing or not depositing a seed layer, electroplating and filling a metal material in the deep hole to remove redundant metal materials on the surface of the silicon substrate, then depositing an insulating material on the surface of the silicon substrate by using an RDL process, specifically, coating photoresist on the insulating material, exposing, developing to form an RDL circuit pattern, sputtering and depositing and/or electroplating metallic copper in the RDL circuit pattern to form an interconnection line, forming an intermediate connecting layer, stripping the photoresist, and obtaining the TSV intermediate layer.
2. The method for manufacturing the multi-chip connecting structure according to claim 1, wherein the step of temporary bonding comprises the steps of symmetrically arranging every two HBM Die on two sides of one SOC Die by using a bonding machine, bonding the copper stud bumps of the HBM Die and the SOC Die face down with the bonding layer, and controlling the depth of embedding the copper stud bumps into the bonding layer to be 2-3 μm, wherein the total number of the HBM Die is more than or equal to 2, and the total number of the SOC Die is more than or equal to 1.
3. The method of manufacturing a multi-chip connection structure according to claim 1, wherein the metal pad of the SOC Die has copper stud bumps having a height of 4-8 μm and a width of 5-25 μm, and the metal pad of the HBM Die has copper stud bumps having a height of 4-8 μm and a width of 5-25 μm.
4. The method of claim 1, wherein the metal material comprises copper when the deep hole is electroplated with the metal material, and wherein the copper-copper bonding is performed between the exposed surface of the copper stud bump and the via interposer when the copper-copper bonding is performed between the exposed surface and the via interposer.
5. The method of fabricating a multi-chip interconnect structure of claim 1, wherein removing excess silicon substrate from the TSV interposer comprises:
The thickness d1 of the redundant silicon substrate is thinned to 3-10 mu m by using a grinder, then the bottom of the silicon substrate is etched by using an etching process, a part of deep hole wrapped by the silicon substrate is exposed, the thickness of the deep hole exposed outside is 1-5 mu m, then a non-metal dielectric material is deposited on two sides of the exposed deep hole by using a PECVD process, and then the bottom of the silicon substrate is flattened by using a CMP process.
6. The method of manufacturing a multi-chip interconnect structure of claim 1 or claim 5, wherein the non-metallic dielectric material comprises at least one of silicon nitride and silicon dioxide.
7. The method of manufacturing a multi-chip interconnect structure of claim 1, wherein constructing a complete RDL layer on the bottom of module two comprises the steps of:
forming a passivation layer at the bottom of the second module, covering the passivation layer by using a mask, exposing, dissolving the passivation layer outside the mask, leaving a designed pattern on the second module, sputtering a titanium layer and a copper layer on the designed pattern to form a PVD layer, and forming a first RDL layer by the PVD layer and the rest passivation layer;
Forming a photoresist layer on the first RDL layer, covering the photoresist layer by using a mask, exposing, dissolving the photoresist layer outside the mask, leaving a designed pattern on the first RDL layer, and electroplating copper on the designed pattern to form a conductive circuit;
Removing the residual photoresist, and reserving a conductive circuit formed by electroplating;
etching to remove unnecessary conductive lines, only retaining the conductive lines connected with the PVD layer, generating a vacant gap after etching, forming a protective layer in the gap, and forming a second RDL layer by the conductive lines and the protective layer;
the first RDL layer and the second RDL layer together form a complete RDL layer.
8. The method for manufacturing a multi-chip connection structure according to claim 1, wherein the parameters of temporary bonding include an initial contact pressure of 0.5-1.0MPa, copper stud bumps in contact with the adhesive layer but not embedded, an embedding stage pressure of 2.5-3.5MPa, a control portion of copper stud bumps embedded in the adhesive layer, and a dwell time of 8-15 seconds.
9. The method for manufacturing a multi-chip connecting structure according to claim 1, wherein the molding compound is used for plastic packaging, and the preparation of the molding compound comprises the following steps:
bisphenol F type epoxy resin and reactive diluent are uniformly mixed to obtain resin mixed solution,
Uniformly mixing large-size silicon dioxide, small-size silicon dioxide and nano particles to obtain mixed powder;
slowly adding the resin mixed solution into the mixed powder, and stirring to obtain a mixture;
adding an antifoaming agent and a leveling agent into the mixture, and stirring to obtain a mixed solution;
slowly adding the curing agent into the mixed solution, stirring, and vacuum defoaming to obtain a molding compound;
Wherein the particle size of the large-size silica is 10-20 μm, the particle size of the small-size silica is 0.1-0.5 μm, and the reactive diluent comprises siloxane oligomer.