CN121551903A - Self-protection flux-cored wire and production method thereof - Google Patents

Self-protection flux-cored wire and production method thereof

Info

Publication number
CN121551903A
CN121551903A CN202511953578.3A CN202511953578A CN121551903A CN 121551903 A CN121551903 A CN 121551903A CN 202511953578 A CN202511953578 A CN 202511953578A CN 121551903 A CN121551903 A CN 121551903A
Authority
CN
China
Prior art keywords
flux
cored wire
self
forming
powder
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN202511953578.3A
Other languages
Chinese (zh)
Inventor
郎鹤磊
沈峰
周志豪
刘辉
柯九兰
李敏明
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Jinqiao Welding Materials Jiangsu Co ltd
Original Assignee
Jinqiao Welding Materials Jiangsu Co ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jinqiao Welding Materials Jiangsu Co ltd filed Critical Jinqiao Welding Materials Jiangsu Co ltd
Priority to CN202511953578.3A priority Critical patent/CN121551903A/en
Publication of CN121551903A publication Critical patent/CN121551903A/en
Pending legal-status Critical Current

Abstract

The invention discloses a self-protection flux-cored wire and a production method thereof, wherein the preparation method comprises the following steps: S1, material treatment, S2, processing and treatment, S3, quality detection, S4, packaging and transportation. According to the invention, a medicinal powder formula is carefully designed according to the target performance of a welding wire, the formula generally comprises ‌ slag forming agents, ‌ slag forming agents, molten pool protection, molten pool metallurgical reaction control, weld joint forming improvement, ‌ deoxidizing agents, ‌ oxygen and nitrogen removal in the molten pool, air hole and embrittlement prevention, gas forming agents, ‌ thermal decomposition to generate protective gas, gas hood formation at the end of the welding wire to isolate air, alloying agents, alloying elements, which are added into deposited metal, achieve the required chemical components and performance, arc stability improvement of ‌ arc stability, and ‌ binding agents, which are sometimes added with a small amount of binding agents, improve the fluidity of the medicinal powder or keep the shape after filling, thereby improving the application range of the flux-cored welding wire, being applicable to various working environments and improving the production quality of the flux-cored wire.

Description

Self-protection flux-cored wire and production method thereof
Technical Field
The invention relates to the technical field of flux-cored wires, in particular to a self-protection flux-cored wire and a production method thereof.
Background
The welding wire is used as a metal wire for filling metal or conducting an electric arc during welding, a welding line is formed after the welding wire is melted to be connected with a workpiece, the flux-cored wire is a welding material for filling the flux-cored material in a pipe, the gas slag is used for jointly protecting a molten pool ‌, the welding wire has the characteristics of stable electric arc, attractive molding and high deposition efficiency, the flux core provides the functions of arc stabilization and slag formation, a gas and slag double protection layer is formed, and the tensile strength is superior to that of a solid welding wire ‌, so that the flux-cored wire which is poor in original filling effect, simple and rapid in manufacturing process is difficult to finish the existing high-quality and rapid manufacturing process, and is characterized by the following aspects:
The method comprises the steps of (1) preparing flux-cored wires with different properties due to single material and incapability of preparing the flux-cored wires with different working environments, so that the preparation quality of the flux-cored wires is reduced, (2) detecting the whole preparation flow during preparation of the flux-cored wires, so that the environmental friendliness in the preparation process is reduced, and (3) detecting the rough appearance of the flux-cored wires after the preparation of the flux-cored wires is finished, and comprehensively detecting the chemical components, the service life and the weather resistance of the flux-cored wires, so that the defective rate of the flux-cored wires is improved.
Disclosure of Invention
The invention aims to provide a self-protection flux-cored wire and a production method thereof, which aim to solve the problems that (1) when the flux-cored wire is prepared by the prior flux-cored wire, the flux-cored wire with different properties cannot be manufactured in different working environments due to single material, so that the preparation quality of the flux-cored wire is reduced, (2) when the flux-cored wire is prepared, the whole preparation process cannot be checked, so that the environmental protection performance in the preparation process is reduced, and (3) after the preparation of the flux-cored wire is finished, only rough appearance detection is carried out, and the chemical components, the service life and the weather resistance of the flux-cored wire cannot be comprehensively detected, so that the defective rate of the flux-cored wire is improved.
In order to achieve the purpose, the invention provides the following technical scheme that the production method of the self-protection flux-cored wire comprises the following steps:
S1, material treatment
S1.1, preparing a steel belt, ① selecting raw materials, ② uncoiling and cleaning, ③ longitudinal shearing, S1.2, forming the steel belt, conveying the cleaned narrow steel belt into a ‌ forming unit ‌, S1.3, preparing medicinal powder, ① designing a formula, and processing a slag former, a deoxidizer, a gas former, an alloy agent, an arc stabilizer, a binder, ② powder, ③ filling, and S1.4, and closing and initially compacting ‌;
S2, processing and treating
S2.1, drawing reducing, ① finish rolling, ② straightening, ③ surface treatment, S2.2, winding the finished product, S2.3 and sealing and packaging ‌;
S3, quality detection
S3.1, raw material inspection, namely, component, size, moisture and cleanliness of steel belts and powder raw materials, S3.2, process monitoring, forming size, filling rate, closing quality, drawing size tolerance, surface quality, winding quality, S3.3, final product inspection, ① appearance inspection, diameter, ovality, surface defect, ② chemical component analysis, cladding metal, ③ welding process performance test, arc stability, splashing size, ④ cladding metal mechanical performance test, tensile strength, yield strength and ⑤ diffusion hydrogen content detection;
s4, packaging and transporting
S4.1, packaging, cleaning, ①, dedusting, ② drying, ③ sterilization, S4.2, product transportation, product fixation and storage to a drying place.
A self-protection flux-cored wire comprises 48% of metal powder mixture, 42% of slag former, 2% of deoxidizer, 3% of gas former, 1% of alloy agent, 3% of arc stabilizer and 1% of binder.
Preferably, the dry powder filled in the step S1 is uniformly, continuously and stably filled into the cavity of the forming steel belt by the ‌ powder filling machine ‌.
Preferably, the filling process in step S1 is performed in a dry, low humidity environment.
Preferably, the drawing reduction ratio calculation formula is ra= (a) 0-A1)/A0 100, Wherein A 0 is the cross-sectional area of the welding wire before drawing in the calculation formula, the unit is mm2, and A 1 is the cross-sectional area of the welding wire after drawing in the unit of mm2.
Preferably, the calculation formula n=k of the number of times of forming the steel strip(H 0 -Hf)/t, wherein n is the minimum number of forming channels, H 0 is the initial width of the raw material strip, hf is the final section development width in mm, t is the material thickness in mm, and k is the complexity factor.
Preferably, when the k is a coefficient, the simple section is 0.8-1.2, and the complex section is 1.5-2.5.
Preferably, the single-pass bending moment m=σy in the steel strip formingbt2/6K。
Preferably, σy in the formula is the material yield strength, the unit is MPa, b is the width of the bending region, the unit is mm, t is the material thickness, the unit is mm, K is a correction coefficient, 1.2-1.5 is taken, and the hardening effect is considered.
Compared with the prior art, the invention has the beneficial effects that:
1. According to the invention, a medicinal powder formula is carefully designed according to the target performance of a welding wire, the formula generally comprises ‌ slag forming agents, ‌ slag forming agents, molten pool protection, molten pool metallurgical reaction control, weld joint forming improvement, ‌ deoxidizing agents, ‌ oxygen and nitrogen removal in the molten pool, air hole and embrittlement prevention, gas forming agents, ‌ thermal decomposition to generate protective gas, gas hood formation at the end of the welding wire to isolate air, alloying agents, alloying elements, which are added into deposited metal, achieve the required chemical components and performance, arc stability improvement of ‌ arc stability, and ‌ binding agents, which are sometimes added with a small amount of binding agents, improve the fluidity of the medicinal powder or keep the shape after filling, thereby improving the application range of the flux-cored welding wire, being applicable to various working environments and improving the production quality of the flux-cored wire.
2. According to the invention, a strict quality control point is arranged in each key working procedure of production, components, sizes, moisture and cleanliness of steel strips and medicinal powder raw materials are carried out on raw materials, then detection effects are carried out on forming sizes, filling rates, closing quality, drawing dimensional tolerance, surface quality and winding quality remotely, and in the preparation process, harmful substances in waste gas and air in the production process are detected, so that the detection effect on the environment in the production process is carried out, and the environmental protection performance in the production process is ensured.
3. According to the invention, the final product is inspected, the appearance of the product is subjected to diameter, ellipticity and surface defect detection, then the chemical composition analysis of the product is utilized by utilizing deposited metal, then the arc stability, splashing size, deslagging performance and smoke dust of the product are tested by utilizing welding process performance, and then the tensile strength, yield strength, elongation and impact toughness of the product are tested by utilizing the mechanical property of the deposited metal, so that the product can be comprehensively subjected to detection, and the defective rate of product production is reduced.
Drawings
FIG. 1 is a flow chart of a method of producing a high rust resistant flux-cored wire of the present invention;
FIG. 2 is a graph of the composition content of the high rust resistance flux-cored wire of the invention;
FIG. 3 is a partial logic code diagram of a forming unit in the method of producing a high rust resistant flux-cored wire of the invention.
Detailed Description
The following description of the embodiments of the present invention will be made clearly and completely with reference to the accompanying drawings, in which it is apparent that the embodiments described are only some embodiments of the present invention, but not all embodiments. All other embodiments, which can be made by those skilled in the art based on the embodiments of the invention without making any inventive effort, are intended to be within the scope of the invention.
Embodiment one:
Referring to fig. 1-3, a method for producing a self-shielded flux-cored wire includes the following steps:
S1, material treatment
S1.1, preparing a steel belt; ① raw material selection; ② uncoiling and cleaning; ③ slitting, S1.2, steel strip shaping, clean narrow steel strip is sent to ‌ shaping unit ‌, S1.3, powder preparation, ① formulation design, slag former, deoxidizer, gas former, alloy, arc stabilizer, binder, ② powder processing, ③ filling, S1.4, closing initial compaction, working personnel select cold rolled steel strip of low alloy steel with specific components, width, thickness and surface quality of the steel strip are vital, large coil steel strip is uncoiled, oil stain and rust on the surface are removed by a cleaning device, ensuring reliable combination of subsequent procedures and powder purity, then the wide steel strip is split into narrow strips with required width in a longitudinal direction according to the requirement of final welding wire diameter, then the clean narrow steel strip is sent to ‌ shaping unit ‌, the steel strip is gradually bent into a specific cross-section shape through a series of precision rollers to form an open tubular structure for containing powder, the shaping process requires extremely high precision control, self-guaranteeing the stability of the subsequent filling and closing, the core technology is that the welding wire is protected, the welding wire is well-covered by the oxygen-protecting film, the welding wire is well-covered by the welding wire, the oxygen-protecting agent is well contained in the welding wire formulation, the welding wire is well-covered by the welding wire, the welding flux is well-covered by the welding wire, the welding flux is well, the welding wire is well is kept in the welding wire is well, the welding well is kept in the welding alloy is well, the welding wire is well is covered with the welding alloy is well, the welding wire is well, the welding alloy is well is easy, the welding alloy is easy, the welding is the welding alloy is the welding steel is the welding steel the steel is the steel is the steel the, the application range of the flux-cored wire is improved, the flux-cored wire is suitable for various working environments, the production quality of the flux-cored wire is improved, various raw materials are weighed according to an accurate proportion, are uniformly mixed, generally need to be crushed and ground to a specified granularity, are strictly dried to remove moisture, the accurately measured dry powder is uniformly, continuously and stably filled into a pipe cavity of a formed steel belt through a ‌ powder filling machine ‌, the opening type steel belt filled with the powder immediately enters a ‌ closed roller ‌, the edges of the opening type steel belt are tightly rolled together by the closed roller, the powder is completely sealed in the pipe cavity formed by the steel belt, meanwhile, the powder in the pipe cavity is preliminarily compacted in the closing process, gaps are reduced, and the filling density and uniformity ‌ are improved;
S2, processing and treating
S2.1, drawing reducing, ① finish rolling, ② straightening, ③ surface treatment, S2.2, winding finished products, S2.3, sealing and packaging, wherein a closed welding wire blank enters a ‌ drawing unit ‌, the welding wire blank passes through a series of ‌ wire drawing dies which are gradually reduced, the diameter of the welding wire is gradually reduced to be close to the final required target size under the action of strong drawing force and lubricant, the steel strip material is plastically deformed and hardened in the drawing process, meanwhile, the internal medicinal powder is further compacted, the finish rolling process is added after the drawing in part of the process, so that the welding wire obtains more accurate diameter tolerance, more round cross-section shape and smoother surface, the bending generated in the drawing is eliminated, the welding wire is straightened, then slight polishing or cleaning is carried out, the residual drawing lubricant and other pollutants on the surface are removed, the continuous finishing welding wire is wound on a welding wire reel according to the weight required by a client, the winding is required to ensure that the winding is neat, compact, no cross-connection and no compression injury are ensured, and ‌ is fed during welding;
S3, quality detection
S3.1, raw material inspection, steel belt, composition, size, moisture and cleanliness of powder raw materials, S3.2, process monitoring, forming size, filling rate, closing quality, drawing size tolerance, surface quality, winding quality, S3.3, final product inspection, ① appearance inspection, diameter, ovality, surface defect, ② chemical composition analysis, cladding metal, ③ welding process performance test, arc stability, splashing size, ④ cladding metal mechanical performance test, tensile strength, yield strength, ⑤ diffusion hydrogen content test, each key process of production is provided with a strict quality control point, steel belt, composition, size, moisture and cleanliness of powder raw materials are detected on the raw materials, then the forming size, filling rate, closing quality, drawing size tolerance, surface quality and winding quality are detected remotely, in the preparation process, waste gas and harmful substances in the air are detected in the production process, thereby the environment is detected in the production process, environment is ensured, the environment protection performance in the production process is checked, the final product inspection is carried out, the appearance diameter, the surface defect detection, the tensile strength and the surface defect detection function of the products are carried out, the product is then the impact performance test is carried out on the appearance diameter, the tensile strength and the product, the overall welding process performance is reduced, the product is fully tested by using the tensile strength and the tensile strength, the product is then fully tested, the welding process performance is reduced, the overall stability is reduced;
s4, packaging and transporting
S4.1, packaging is clean, ① is dedusted, ② is dried, ③ is sterilized, S4.2, products are transported, the products are fixed and stored in a dry place, because the medicine powder of the self-protection flux-cored wire is easy to absorb moisture, serious air holes, splash increase and unstable electric arc are generated during welding after the medicine powder absorbs moisture, a wire reel after winding must be immediately put into ‌ sealed packages with high-efficiency moisture-proof material built-in desiccant bags and aluminum foil moisture-proof films, and ‌ is usually a vacuum sealed and inert gas filled plastic bag, so that the packages are ensured to be always kept in a sealed state before transportation and storage until use.
A self-protection flux-cored wire comprises 48% of metal powder mixture, 42% of slag former, 2% of deoxidizer, 3% of gas former, 1% of alloy agent, 3% of arc stabilizer and 1% of binder.
In this embodiment, the dry powder filled in the step S1 is uniformly, continuously and stably filled into the cavity of the forming steel belt by the ‌ powder filling machine ‌.
In this embodiment, the filling process in step S1 is performed in a dry, low humidity environment.
In the embodiment, the drawing reduction ratio calculation formula is RA= (A) 0-A1)/A0 100, Wherein A 0 is the cross-sectional area of the welding wire before drawing in the calculation formula, the unit is mm2, and A 1 is the cross-sectional area of the welding wire after drawing in the unit of mm2.
In the embodiment, the calculation formula n=k of the number of times of forming the steel strip(H 0 -Hf)/t, wherein n is the minimum number of forming channels, H 0 is the initial width of the raw material strip, hf is the final section development width in mm, t is the material thickness in mm, and k is the complexity factor.
In the embodiment, when the k is a coefficient, the simple section is 0.8-1.2, and the complex section is 1.5-2.5.
In this example, the single pass bending moment m=σy in the strip formingbt2/6K。
In the embodiment, sigma y in the formula is the yield strength of the material, the unit is MPa, b is the width of a bending area, the unit is mm, t is the thickness of the material, the unit is mm, K is a correction coefficient, 1.2-1.5 is taken, and the hardening effect is considered.
Embodiment two:
As shown in the figure, unlike the first embodiment, the self-shielded flux-cored wire and the production method thereof according to the present embodiment include the following steps:
S1, material treatment
S1.1, preparing a steel belt, ① selecting raw materials, ② uncoiling and cleaning, ③ longitudinal shearing, S1.2, forming the steel belt, conveying the cleaned narrow steel belt into a ‌ forming unit ‌, S1.3, preparing medicinal powder, ② processing the powder, ③ filling, and S1.4 closing and primary compacting.
S2, processing and treating
S2.1, drawing reducing, ① finish rolling, ② straightening, ③ surface treatment, S2.2, winding the finished product, S2.3 and sealing and packaging.
S3, quality detection
S3.1, inspecting a final product, carrying out ① appearance inspection, diameter, ovality, surface defects, S3.2 chemical component analysis, cladding metal, S3.3 welding process performance test, arc stability and splash size.
S4, packaging and transporting
S4.1, cleaning package, ① dedusting, ② drying, ③ sterilization, S4.2, product transportation, product fixation and storage to a drying place, wherein the powder of the self-protection flux-cored wire is easy to absorb moisture, so that the problems of serious air holes, increased splashing and unstable electric arc are caused during welding after the moisture absorption, and a coiled wire reel must be immediately filled into ‌ sealed package with a high-efficiency moisture-proof material built-in desiccant bag and an aluminum foil moisture-proof film.
In summary, in comparison with the first embodiment and the second embodiment, according to the target performance of the welding wire, the powder formulation is carefully designed, the formulation generally comprises ‌ a slag former ‌ to form slag, protect a molten pool, control the metallurgical reaction of the molten pool, improve the weld formation, a deoxidizer ‌ removes oxygen and nitrogen in the molten pool, prevent air holes and embrittlement, a gas former ‌ is heated and decomposed to generate protective gas, a gas hood is formed at the end of the welding wire to isolate air, an alloying element is added into deposited metal to achieve the required chemical components and performance, an arc stabilizer ‌ improves the arc stability, a small amount of binder ‌ is sometimes added to improve the fluidity of the powder or maintain the shape after filling, thereby improving the application range of the flux-cored wire, being applicable to various working environments and improving the production quality of the flux-cored wire.
It is noted that relational terms such as first and second, and the like are used solely to distinguish one entity or action from another entity or action without necessarily requiring or implying any actual such relationship or order between such entities or actions. Moreover, the terms "comprises," "comprising," or any other variation thereof, are intended to cover a non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements does not include only those elements but may include other elements not expressly listed or inherent to such process, method, article, or apparatus.
Although embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made therein without departing from the principles and spirit of the invention, the scope of which is defined in the appended claims and their equivalents.

Claims (9)

1. The production method of the self-protection flux-cored wire is characterized by comprising the following steps of:
S1, material treatment
S1.1, preparing a steel belt, ① selecting raw materials, ② uncoiling and cleaning, ③ longitudinal shearing, S1.2, forming the steel belt, conveying the cleaned narrow steel belt into a ‌ forming unit ‌, S1.3, preparing medicinal powder, ① designing a formula, and processing a slag former, a deoxidizer, a gas former, an alloy agent, an arc stabilizer, a binder, ② powder, ③ filling, and S1.4, and closing and initially compacting ‌;
S2, processing and treating
S2.1, drawing reducing, ① finish rolling, ② straightening, ③ surface treatment, S2.2, winding the finished product, S2.3 and sealing and packaging ‌;
S3, quality detection
S3.1, raw material inspection, namely, component, size, moisture and cleanliness of steel belts and powder raw materials, S3.2, process monitoring, forming size, filling rate, closing quality, drawing size tolerance, surface quality, winding quality, S3.3, final product inspection, ① appearance inspection, diameter, ovality, surface defect, ② chemical component analysis, cladding metal, ③ welding process performance test, arc stability, splashing size, ④ cladding metal mechanical performance test, tensile strength, yield strength and ⑤ diffusion hydrogen content detection;
s4, packaging and transporting
S4.1, packaging, cleaning, ①, dedusting, ② drying, ③ sterilization, S4.2, product transportation, product fixation and storage to a drying place.
2. A self-protection flux-cored wire based on the production method of claim 1 is characterized by comprising 48% of a medicament formula, 48% of a metal powder mixture, 42% of a slag former, 2% of a deoxidizer, 3% of a gas former, 1% of an alloy agent, 3% of an arc stabilizer and 1% of a binder.
3. The method of claim 1, wherein the dry powder is uniformly, continuously and stably filled into the cavity of the forming steel strip by a ‌ powder filling machine ‌.
4. The method of claim 1, wherein the filling step S1 is performed in a dry, low humidity environment.
5. The method for producing a self-shielded flux-cored wire according to claim 1, wherein the drawing reduction ratio calculation formula is RA= (A) 0-A1)/A0 100, Wherein A 0 is the cross-sectional area of the welding wire before drawing in the calculation formula, the unit is mm2, and A 1 is the cross-sectional area of the welding wire after drawing in the unit of mm2.
6. The method for producing a self-shielded flux-cored wire according to claim 1, wherein the number of steel strip forming passes is calculated by a formula n=k(H 0 -Hf)/t, wherein n is the minimum number of forming channels, H 0 is the initial width of the raw material strip, hf is the final section development width in mm, t is the material thickness in mm, and k is the complexity factor.
7. The method for producing the self-shielded flux-cored wire according to claim 6, wherein the k coefficient is 0.8-1.2 in simple section and 1.5-2.5 in complex section.
8. The method for producing a self-shielded flux-cored wire according to claim 1, wherein the single-pass bending moment M=σy in the forming of the steel stripbt2/6K。
9. The method for producing the self-shielded flux-cored wire according to claim 8, wherein σy is a material yield strength in MPa, b is a bending area width in mm, t is a material thickness in mm, K is a correction coefficient, 1.2-1.5 is taken, and a hardening effect is considered.
CN202511953578.3A 2025-12-23 2025-12-23 Self-protection flux-cored wire and production method thereof Pending CN121551903A (en)