CN121574499A - A temperature-resistant multifunctional epoxy resin and its preparation method - Google Patents

A temperature-resistant multifunctional epoxy resin and its preparation method

Info

Publication number
CN121574499A
CN121574499A CN202610096106.9A CN202610096106A CN121574499A CN 121574499 A CN121574499 A CN 121574499A CN 202610096106 A CN202610096106 A CN 202610096106A CN 121574499 A CN121574499 A CN 121574499A
Authority
CN
China
Prior art keywords
epoxy resin
multifunctional epoxy
parts
heat
resistant multifunctional
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
CN202610096106.9A
Other languages
Chinese (zh)
Inventor
原宇航
陈耀兵
张桦
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hubei Gemvon New Material Co ltd
Original Assignee
Hubei Gemvon New Material Co ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hubei Gemvon New Material Co ltd filed Critical Hubei Gemvon New Material Co ltd
Priority to CN202610096106.9A priority Critical patent/CN121574499A/en
Publication of CN121574499A publication Critical patent/CN121574499A/en
Withdrawn legal-status Critical Current

Abstract

The application discloses a temperature-resistant multifunctional epoxy resin and a preparation method thereof. On one hand, the application provides a temperature-resistant multifunctional epoxy resin, which comprises, by mass, 100 parts of AFG-90 multifunctional epoxy resin, 20-40 parts of epoxy-terminated polyphenyl ether, 8-16 parts of epoxy modified silicone oil and 6-12 parts of hydrophobic fumed silica. On the other hand, the application provides a preparation method of the temperature-resistant multifunctional epoxy resin. The glass transition temperature of the application exceeds 240 ℃, and the application has relatively excellent temperature resistance, excellent moisture resistance and extremely low water absorption.

Description

Temperature-resistant multifunctional epoxy resin and preparation method thereof
Technical Field
The application relates to the technical field of electronic packaging materials, in particular to a temperature-resistant multifunctional epoxy resin and a preparation method thereof.
Background
The preparation of electronic components is the basis of the electronics industry, and packaging technology is critical to ensure proper operation of the electronic components. Along with the development of electronic equipment towards miniaturization, light weight and high performance, people put forward higher requirements on packaging technology, promote the continuous development of packaging materials, and meanwhile, promote the development of packaging materials, and gradually change from metal packaging materials and ceramic packaging materials to plastic packaging materials, wherein the epoxy plastic packaging materials occupy more than 97% of market of microelectronic packaging materials due to the advantages of high reliability, low cost, simple process and the like, and are widely applied to various packaging fields of semiconductor devices, integrated circuits, consumer electronics, automobiles, aerospace, military and the like.
The epoxy plastic package material consists of epoxy resin, various fillers and various assistants, and has the functions of strengthening the integrity of the electronic device, improving the resistance to external impact and vibration, improving the insulation between internal elements and circuits, being beneficial to the miniaturization and the light weight of the device, avoiding the direct exposure of the elements and the circuits, improving the waterproof and dampproof performances of the device and the like. Wherein, the epoxy resin is used as the base material of the packaging material and is the core for determining the performance of the packaging material.
With the development of the electronic industry, the performance requirements on various electronic components are higher, correspondingly, the working temperatures of various electronic components are also increased, and the working temperatures of the existing various electronic components, such as common industrial chips, computer processors and the like, are relatively higher. The epoxy resin material has insufficient high temperature resistance, which is a big defect of being used as an electronic component packaging material. The prior art researches show that the improvement of the crosslinking density of the epoxy resin can effectively improve the glass transition temperature and further improve the high temperature resistance of the epoxy resin, but the improvement of the crosslinking density can improve the hygroscopicity of the epoxy resin material, and the moisture resistance is insufficient, so that the packaged electronic component has the problems of cracking, layering and the like under the high-temperature working condition, and the electronic component short circuit can be seriously even caused.
Therefore, designing an epoxy resin material with relatively good high temperature resistance and excellent moisture resistance is a technical problem to be solved in the field.
Disclosure of Invention
In order to solve at least one technical problem, an epoxy resin material with a glass transition temperature of more than 240 ℃ and relatively excellent temperature resistance, excellent moisture resistance and extremely low water absorption is developed, and the application provides a temperature-resistant multifunctional epoxy resin and a preparation method thereof.
On one hand, the application provides a temperature-resistant multifunctional epoxy resin, which comprises, by mass, 100 parts of AFG-90 multifunctional epoxy resin, 20-40 parts of epoxy-terminated polyphenyl ether, 8-16 parts of epoxy modified silicone oil and 6-12 parts of hydrophobic fumed silica.
Optionally, the temperature-resistant multifunctional epoxy resin comprises, by mass, 100 parts of AFG-90 multifunctional epoxy resin, 24-28 parts of epoxy-terminated polyphenyl ether, 10-12 parts of epoxy modified silicone oil and 8-10 parts of hydrophobic fumed silica.
Optionally, the preparation of the epoxy-capped polyphenylene ether comprises the following steps:
s1-a, mixing dihydroxy-terminated polyphenyl ether and epichlorohydrin according to a mass ratio of 10:6.8-7.2, adding toluene for dissolution, and then adding quaternary ammonium salt, sodium hydroxide and a 15-crown ether-5 catalyst to prepare a reaction solution;
s1-b, reacting the reaction solution prepared in the step S1-a for more than 3 hours at the temperature of 70-75 ℃ under the protection of nitrogen, standing, cooling to normal temperature, and filtering by a nanofiltration membrane to obtain filtrate;
S1-C, distilling the filtrate obtained in the step S1-b at 100-105 ℃ under reduced pressure to remove the 15-crown ether-5 catalyst, adding the catalyst into methanol for crystallization, filtering out the crystallization, washing with water, and drying to obtain the epoxy-terminated polyphenyl ether.
Further optionally, in the step S1-a, the addition amount of the quaternary ammonium salt accounts for 3-5% of the total mass of the dihydroxy-terminated polyphenyl ether and the epichlorohydrin.
Further optionally, in the step S1-a, the addition amount of the sodium hydroxide accounts for 8-10% of the total mass of the dihydroxy-terminated polyphenyl ether and the epichlorohydrin.
Further optionally, in the step S1-a, the addition amount of the 15-crown ether-5 catalyst accounts for 2-4% of the total mass of the dihydroxy-terminated polyphenyl ether and the epichlorohydrin.
Further alternatively, in the step S1-b, after the nanofiltration membrane is filtered, the filtrate is subjected to dechlorination treatment by using a bimetal oxide of calcium oxide and aluminum oxide.
Optionally, the preparation of the epoxy modified silicone oil comprises the following steps:
S2-a, mixing 4-vinylphenyl glycidyl ether and hydrogen-terminated polydimethylsiloxane according to a molar ratio of not less than 2.1:1, and adding an Ashby' S catalyst to prepare a reaction solution;
s2-b, pre-reacting the reaction solution prepared in the step S2-a for more than 1h at the temperature of 60-65 ℃, and then heating to 90-95 ℃ for more than 4.5h to obtain a reaction mixed solution;
S2-C, decoloring the reaction mixed solution obtained in the step S2-b by using active carbon, filtering and removing the active carbon by filtering, and distilling at 120-125 ℃ under reduced pressure to remove unreacted 4-vinylphenyl glycidyl ether to obtain the epoxy modified silicone oil.
Further alternatively, in the step S2-a, the molar ratio of the 4-vinylphenyl glycidyl ether to the hydrogen-terminated polydimethylsiloxane is 2.2-2.4:1.
On the other hand, the application provides a preparation method of the temperature-resistant multifunctional epoxy resin, which comprises the following steps:
s1, preparing epoxy-terminated polyphenyl ether;
S2, preparing epoxy modified silicone oil;
And S3, precisely weighing the raw materials of the components according to the proportion, mixing, and placing the mixture in a vacuum drying oven for curing reaction at 95-105 ℃ for more than 1.5 hours to prepare the temperature-resistant multifunctional epoxy resin.
In summary, the present invention includes at least one of the following beneficial technical effects:
1. According to the application, AFG-90 multifunctional epoxy resin is used as a main raw material, a certain amount of epoxy end-capped polyphenyl ether and epoxy modified silicone oil are added, and the crosslinking density of the epoxy resin can be effectively improved based on the difference of the molecular weights of the epoxy end-capped polyphenyl ether and the epoxy modified silicone oil, so that the temperature resistance of the epoxy resin is effectively improved; in addition, the polyphenylene oxide functional groups and specific organic silicon functional groups are introduced into the resin, so that the toughness and impact strength of the epoxy resin can be effectively improved, the molecular structure of the epoxy resin can be effectively changed, and the glass transition temperature of the cured epoxy resin can be effectively improved due to the introduction of a plurality of functional groups.
2. According to the application, the hydrophobic fumed silica is added into the epoxy resin system, so that the silica group can be introduced into the system in addition to the filler auxiliary agent, and the glass transition temperature of the cured epoxy resin is further improved.
3. According to the epoxy resin, the polyphenyl ether and the organic silicon functional groups are introduced, so that the hydrophobicity of the epoxy resin can be greatly improved on the premise of greatly improving the temperature resistance of the epoxy resin, the moisture absorption rate of the cured epoxy resin is effectively reduced, and the moisture resistance is greatly improved.
Detailed Description
The present application will be described in further detail with reference to examples.
The application provides a temperature-resistant multifunctional epoxy resin, which comprises, by mass, 100 parts of AFG-90 multifunctional epoxy resin, 20-40 parts of epoxy-terminated polyphenyl ether, 8-16 parts of epoxy modified silicone oil and 6-12 parts of hydrophobic fumed silica.
The preparation method of the temperature-resistant multifunctional epoxy resin comprises the following steps:
s1, preparing epoxy-terminated polyphenyl ether;
S2, preparing epoxy modified silicone oil;
And S3, precisely weighing the raw materials of the components according to the proportion, mixing, and placing the mixture in a vacuum drying oven for curing reaction at 95-105 ℃ for more than 1.5 hours to prepare the temperature-resistant multifunctional epoxy resin.
Before the application, the temperature-resistant epoxy resin prepared in the prior art takes the epoxy resin with the multi-phenolic functional group as the main material, the cross-linking density of the cured resin is improved through the multi-functional group, and a large number of benzene ring groups are introduced into the multi-phenolic functional group, so that the glass transition temperature of the epoxy resin can be effectively improved, and the better temperature resistance of the epoxy resin is ensured.
However, the conventional temperature-resistant epoxy resin has insufficient high-temperature moisture resistance and certain hygroscopicity at high temperature, and is used as an epoxy plastic packaging material of electronic components, so that various problems are easy to occur. Although moisture resistance can be improved to some extent by improving the curing agent, the effect is limited and the difficulty of the curing process is significantly increased.
The applicant designs a specific epoxy resin raw material proportion, introduces a plurality of new functional groups of epoxy raw materials, and effectively solves the problems existing in the prior art.
The following are preparation examples and examples of the present application.
The main raw materials selected in the examples of the present application are all commercially available.
The multifunctional epoxy resin is prepared from AFG-90, which is purchased from Shanghai Hua Yi resin Co., ltd, hydrogen-terminated polydimethylsiloxane with purity of 99%, 4-vinylphenyl glycidyl ether with purity of 98%, which is purchased from Hubei Xinghangxingxiao biological technology Co., ltd, ashby's catalyst, which is purchased from Guangzhou Si-you New technology Co., ltd, BY-5000 YC/PT-5000V, dihydroxy-terminated polyphenyl ether, saint base SA90, which is obtained from Dongguan gold particle plastic raw material Co., ltd, epichlorohydrin, jinan chemical Co., ltd, 15-crown ether-5 catalyst, which is purchased from Wuji Xinyi biological technology Co., ltd, and DDS curing agent, which is purchased from Shenyan Xisha material Co., ltd.
The following is a preparation example of the present application.
Preparation example 1
The preparation of the epoxy-terminated polyphenyl ether of the preparation example comprises the following steps:
s1-a, mixing dihydroxy-terminated polyphenyl ether and epichlorohydrin in a mass ratio of 10:6.8, adding toluene until the mixture is just completely dissolved, and then respectively adding tetrabutylammonium bromide accounting for 3 percent of the total mass of the dihydroxy-terminated polyphenyl ether and the epichlorohydrin, sodium hydroxide accounting for 8 percent and 15-crown ether-5 catalyst accounting for 2 percent to prepare a reaction solution;
S1-b, reacting the reaction solution prepared in the step S1-a for 3 hours at 70-75 ℃ under the protection of nitrogen, standing and cooling to normal temperature, filtering by a nanofiltration membrane, adding a bimetallic oxide of calcium oxide and aluminum oxide accounting for 200% of the total mass of the dihydroxyl-terminated polyphenyl ether and the epichlorohydrin in a mass ratio of 3:1, electrifying and dechlorinating by 220V alternating current for 5min, and filtering the bimetallic oxide to obtain filtrate;
S1-C, distilling the filtrate obtained in the step S1-b at 100-105 ℃ under reduced pressure to remove the 15-crown ether-5 catalyst, adding the catalyst into methanol with the same volume, standing, cooling, crystallizing until no new crystal is generated, filtering out the crystal, washing with water, and drying in vacuum to obtain the epoxy-terminated polyphenyl ether.
Preparation example 2
The preparation of the epoxy-terminated polyphenyl ether of the preparation example comprises the following steps:
S1-a, mixing dihydroxy-terminated polyphenyl ether and epichlorohydrin according to a mass ratio of 10:7, adding toluene for dissolution, and then respectively adding tetrabutylammonium bisulfate accounting for 4% of the total mass of the dihydroxy-terminated polyphenyl ether and the epichlorohydrin, 9% of sodium hydroxide and 3% of a 15-crown ether-5 catalyst to prepare a reaction solution;
S1-b, reacting the reaction solution prepared in the step S1-a for 3 hours at 70-75 ℃ under the protection of nitrogen, standing and cooling to normal temperature, filtering by a nanofiltration membrane, adding a bimetallic oxide of calcium oxide and aluminum oxide accounting for 200% of the total mass of the dihydroxyl-terminated polyphenyl ether and the epichlorohydrin in a mass ratio of 3:1, electrifying and dechlorinating by 220V alternating current for 5min, and filtering the bimetallic oxide to obtain filtrate;
S1-C, distilling the filtrate obtained in the step S1-b at 100-105 ℃ under reduced pressure to remove the 15-crown ether-5 catalyst, adding the catalyst into methanol with the same volume, standing, cooling, crystallizing until no new crystal is generated, filtering out the crystal, washing with water, and drying in vacuum to obtain the epoxy-terminated polyphenyl ether.
Preparation example 3
The preparation of the epoxy-terminated polyphenyl ether of the preparation example comprises the following steps:
S1-a, mixing dihydroxy-terminated polyphenyl ether and epichlorohydrin according to the mass ratio of 10:7.2, adding toluene for dissolution, and then respectively adding triethylammonium chloride accounting for 5% of the total mass of the dihydroxy-terminated polyphenyl ether and the epichlorohydrin, 10% of sodium hydroxide and 4% of a 15-crown ether-5 catalyst to prepare a reaction solution;
S1-b, reacting the reaction solution prepared in the step S1-a for 3 hours at 70-75 ℃ under the protection of nitrogen, standing and cooling to normal temperature, filtering by a nanofiltration membrane, adding a bimetallic oxide of calcium oxide and aluminum oxide accounting for 200% of the total mass of the dihydroxyl-terminated polyphenyl ether and the epichlorohydrin in a mass ratio of 3:1, electrifying and dechlorinating by 220V alternating current for 5min, and filtering the bimetallic oxide to obtain filtrate;
S1-C, distilling the filtrate obtained in the step S1-b at 100-105 ℃ under reduced pressure to remove the 15-crown ether-5 catalyst, adding the catalyst into methanol with the same volume, standing, cooling, crystallizing until no new crystal is generated, filtering out the crystal, washing with water, and drying in vacuum to obtain the epoxy-terminated polyphenyl ether.
Preparation example 4
The preparation of the epoxy modified silicone oil of the preparation example comprises the following steps:
S2-a, mixing 4-vinyl phenyl glycidyl ether and hydrogen end-capped polydimethylsiloxane according to a molar ratio of 2.1:1, and adding an Ashby' S catalyst accounting for 2.5% of the total mass of the 4-vinyl phenyl glycidyl ether and the hydrogen end-capped polydimethylsiloxane to prepare a reaction solution;
S2-b, pre-reacting the reaction solution prepared in the step S2-a for 1h at the temperature of 60-65 ℃, and then heating to 90-95 ℃ for 4.5h to obtain a reaction mixed solution;
S2-C, decoloring the reaction mixed solution obtained in the step S2-b by using active carbon, filtering and removing the active carbon by filtering, and distilling at 120-125 ℃ under reduced pressure to remove unreacted 4-vinylphenyl glycidyl ether to obtain the epoxy modified silicone oil.
Preparation example 5
The preparation of the epoxy modified silicone oil of the preparation example comprises the following steps:
s2-a, mixing 4-vinyl phenyl glycidyl ether and hydrogen end-capped polydimethylsiloxane according to a molar ratio of 2.2:1, and adding an Ashby' S catalyst accounting for 2.5% of the total mass of the 4-vinyl phenyl glycidyl ether and the hydrogen end-capped polydimethylsiloxane to prepare a reaction solution;
S2-b, pre-reacting the reaction solution prepared in the step S2-a for 1.5 hours at the temperature of 60-65 ℃, and then heating to 90-95 ℃ for reacting for 5 hours to obtain a reaction mixed solution;
S2-C, decoloring the reaction mixed solution obtained in the step S2-b by using active carbon, filtering and removing the active carbon by filtering, and distilling at 120-125 ℃ under reduced pressure to remove unreacted 4-vinylphenyl glycidyl ether to obtain the epoxy modified silicone oil.
Preparation example 6
The preparation of the epoxy modified silicone oil of the preparation example comprises the following steps:
S2-a, mixing 4-vinyl phenyl glycidyl ether and hydrogen end-capped polydimethylsiloxane according to a molar ratio of 2.4:1, and adding an Ashby' S catalyst accounting for 2.5% of the total mass of the 4-vinyl phenyl glycidyl ether and the hydrogen end-capped polydimethylsiloxane to prepare a reaction solution;
S2-b, pre-reacting the reaction solution prepared in the step S2-a for 1.5 hours at the temperature of 60-65 ℃, and then heating to 90-95 ℃ for reacting for 5.5 hours to obtain a reaction mixed solution;
S2-C, decoloring the reaction mixed solution obtained in the step S2-b by using active carbon, filtering and removing the active carbon by filtering, and distilling at 120-125 ℃ under reduced pressure to remove unreacted 4-vinylphenyl glycidyl ether to obtain the epoxy modified silicone oil.
The following are examples of the application.
The preparation method of the temperature-resistant multifunctional epoxy resin provided by the embodiment of the application comprises the following steps:
s1, selecting epoxy-terminated polyphenyl ether corresponding to a preparation example;
S2, selecting epoxy modified silicone oil corresponding to the preparation example;
and S3, precisely weighing the raw materials of the components according to the proportion, mixing, and then placing the mixture in a vacuum drying oven for curing reaction for 1.5 hours at the temperature of 95-105 ℃ to prepare the temperature-resistant multifunctional epoxy resin.
Example 1
The temperature-resistant multifunctional epoxy resin comprises, by mass, 100 parts of AFG-90 multifunctional epoxy resin, 20 parts of epoxy-terminated polyphenyl ether, 8 parts of epoxy modified silicone oil and 6 parts of hydrophobic fumed silica.
This example selects the epoxy-terminated polyphenylene ether of preparation example 1 and the epoxy-modified silicone oil of preparation example 4.
Example 2
The temperature-resistant multifunctional epoxy resin comprises, by mass, 100 parts of AFG-90 multifunctional epoxy resin, 40 parts of epoxy-terminated polyphenyl ether, 16 parts of epoxy modified silicone oil and 12 parts of hydrophobic fumed silica.
This example selects the epoxy-terminated polyphenylene ether of preparation example 1 and the epoxy-modified silicone oil of preparation example 4.
Example 3
The temperature-resistant multifunctional epoxy resin comprises, by mass, 100 parts of AFG-90 multifunctional epoxy resin, 24 parts of epoxy-terminated polyphenyl ether, 10 parts of epoxy modified silicone oil and 8 parts of hydrophobic fumed silica.
This example selects the epoxy-terminated polyphenylene ether of preparation example 1 and the epoxy-modified silicone oil of preparation example 4.
Example 4
The temperature-resistant multifunctional epoxy resin comprises, by mass, 100 parts of AFG-90 multifunctional epoxy resin, 28 parts of epoxy-terminated polyphenyl ether, 12 parts of epoxy modified silicone oil and 10 parts of hydrophobic fumed silica.
This example selects the epoxy-terminated polyphenylene ether of preparation example 1 and the epoxy-modified silicone oil of preparation example 4.
Example 5
The temperature-resistant multifunctional epoxy resin comprises, by mass, 100 parts of AFG-90 multifunctional epoxy resin, 26 parts of epoxy-terminated polyphenyl ether, 11 parts of epoxy modified silicone oil and 9 parts of hydrophobic fumed silica.
This example selects the epoxy-terminated polyphenylene ether of preparation example 1 and the epoxy-modified silicone oil of preparation example 4.
Example 6
This example differs from example 5 in that this example selects the epoxy-terminated polyphenylene ether of preparation example 2 and the epoxy-modified silicone oil of preparation example 5.
Example 7
This example differs from example 5 in that this example selects the epoxy-terminated polyphenylene ether of preparation 3 and the epoxy-modified silicone oil of preparation 6.
Example 8
This example differs from example 5 in that this example selects the epoxy-terminated polyphenylene ether of preparation example 2 and the epoxy-modified silicone oil of preparation example 6.
Comparative example 1
EPPN-501 multifunctional epoxy resin from Kagaku Kogyo Co., ltd was used as comparative example 1.
Comparative example 2
This comparative example differs from example 8 in that no hydrophobic fumed silica was added.
Comparative example 3
This comparative example differs from example 8 in that the epoxy-capped polyphenylene ether was replaced with an equivalent amount of AFG-90 multifunctional epoxy resin.
Comparative example 4
This comparative example differs from example 8 in that the epoxy modified silicone oil was replaced with an equivalent amount of AFG-90 multifunctional epoxy resin.
The post-curing properties of the products of examples 1 to 8 and comparative examples 1 to 4 were examined. Wherein the curing agent is DDS curing agent, the mass ratio of the resin to the curing agent is 100:55, and the curing conditions are 130 ℃ per 2h+150 ℃ per 2h+180 ℃ per 2h+200 ℃ per 2h.
Wherein, the tensile strength and the impact strength are detected according to the method described in GB/T2567-2008;
the glass transition temperature is detected according to the method described in GB/T194667.2-2004;
the moisture absorption rate was measured according to the method described in GB/T1034-1998.
The results obtained are shown in Table 1 below.
Table 1 examples 1 to 8 and comparative examples 1 to 4 are shown in the results of the performance test after curing
Tensile Strength (MPa) Impact Strength (kJ/m 2) Glass transition temperature (°c) Moisture absorption Rate (%)
Example 1 94 55.8 249 0.18
Example 2 97 57.4 252 0.16
Example 3 103 57.9 258 0.12
Example 4 102 57.8 259 0.11
Example 5 105 58.1 261 0.10
Example 6 107 58.4 264 0.09
Example 7 108 58.7 265 0.08
Example 8 108 58.9 268 0.06
Comparative example 1 92 50.2 238 2.92
Comparative example 2 99 53.7 236 1.22
Comparative example 3 87 49.6 217 2.38
Comparative example 4 91 50.9 224 1.94
As can be seen from the data in Table 1, the epoxy resin prepared in examples 1 to 8 of the present application has a glass transition temperature higher than that of the epoxy resin prepared in comparative example 1 of the prior art by more than 10 ℃ after curing with the curing agent, has more excellent heat resistance than the conventional multifunctional epoxy resin, has mechanical properties obviously superior to those of the epoxy resin prepared in comparative example 1, and has a moisture absorption rate obviously lower than that of the epoxy resin prepared in comparative example 1.
From the data in Table 1, it can be seen from the comparison of the data in examples 1 to 8 that each performance of the cured epoxy resin can be further improved after the raw material proportion is adjusted, and in addition, the cured epoxy resin in example 8 has the optimal performance, and the prepared raw material has higher purity and lower impurity content, and the resin has better performance.
From the data in Table 1, it can be seen that the resin can have both heat resistance and moisture resistance after three functional groups of polyphenylene ether, organosilicon and siloxane groups are introduced in the application, as compared with the data of comparative examples 2 to 4. Any functional group is deleted, so that a cross-linking system and a functional group system designed by the application are broken, and the performance of the resin is obviously reduced.
The above embodiments are not intended to limit the scope of the application, so that the equivalent changes of the structure, shape and principle of the application are covered by the scope of the application.

Claims (10)

1.一种耐温型多官能团环氧树脂,其特征在于,所述耐温型多官能团环氧树脂各原料组分质量份数配比包括:AFG-90多官能环氧树脂100份,环氧封端聚苯醚20~40份,环氧改性硅油8~16份,以及疏水型气相二氧化硅6~12份。1. A heat-resistant multifunctional epoxy resin, characterized in that the mass ratio of each raw material component of the heat-resistant multifunctional epoxy resin includes: 100 parts of AFG-90 multifunctional epoxy resin, 20-40 parts of epoxy-terminated polyphenylene ether, 8-16 parts of epoxy-modified silicone oil, and 6-12 parts of hydrophobic fumed silica. 2.根据权利要求1所述的耐温型多官能团环氧树脂,其特征在于,所述耐温型多官能团环氧树脂各原料组分质量份数配比包括:AFG-90多官能环氧树脂100份,环氧封端聚苯醚24~28份,环氧改性硅油10~12份,以及疏水型气相二氧化硅8~10份。2. The heat-resistant multifunctional epoxy resin according to claim 1, characterized in that the mass ratio of each raw material component of the heat-resistant multifunctional epoxy resin includes: 100 parts of AFG-90 multifunctional epoxy resin, 24-28 parts of epoxy-terminated polyphenylene ether, 10-12 parts of epoxy-modified silicone oil, and 8-10 parts of hydrophobic fumed silica. 3.根据权利要求1所述的耐温型多官能团环氧树脂,其特征在于,所述环氧封端聚苯醚的制备,包括以下步骤:3. The heat-resistant multifunctional epoxy resin according to claim 1, characterized in that the preparation of the epoxy-terminated polyphenylene ether comprises the following steps: S1-a、将双羟基封端聚苯醚和环氧氯丙烷以10:6.8~7.2的质量比混合,添加甲苯溶解,而后添加季铵盐、氢氧化钠和15-冠醚-5催化剂,配制成反应液;S1-a. Dihydroxy-terminated polyphenylene ether and epichlorohydrin are mixed in a mass ratio of 10:6.8~7.2, toluene is added to dissolve them, and then quaternary ammonium salt, sodium hydroxide and 15-crown ether-5 catalyst are added to prepare a reaction solution. S1-b、将步骤S1-a配置的反应液,在氮气保护下,在70~75℃温度下反应3h以上,静置降温至常温,纳滤膜过滤后,得到滤液;S1-b: The reaction solution prepared in step S1-a is reacted at 70~75℃ for more than 3 hours under nitrogen protection, allowed to stand and cool to room temperature, and then filtered through a nanofiltration membrane to obtain the filtrate. S1-c、将步骤S1-b得到的滤液,100~105℃减压蒸馏去除15-冠醚-5催化剂,而后添加至甲醇中结晶,过滤滤出结晶后,水洗、干燥,制得环氧封端聚苯醚。S1-c: The filtrate obtained in step S1-b is subjected to vacuum distillation at 100~105℃ to remove the 15-crown ether-5 catalyst, and then added to methanol for crystallization. After filtering out the crystals, the solution is washed with water and dried to obtain epoxy-terminated polyphenylene ether. 4.根据权利要求3所述的耐温型多官能团环氧树脂,其特征在于,所述步骤S1-a中,季铵盐的添加量占双羟基封端聚苯醚和环氧氯丙烷总质量的3~5%。4. The heat-resistant multifunctional epoxy resin according to claim 3, characterized in that, in step S1-a, the amount of quaternary ammonium salt added accounts for 3-5% of the total mass of dihydroxy-terminated polyphenylene ether and epichlorohydrin. 5.根据权利要求3所述的耐温型多官能团环氧树脂,其特征在于,所述步骤S1-a中,氢氧化钠的添加量占双羟基封端聚苯醚和环氧氯丙烷总质量的8~10%。5. The heat-resistant multifunctional epoxy resin according to claim 3, characterized in that, in step S1-a, the amount of sodium hydroxide added accounts for 8-10% of the total mass of dihydroxy-terminated polyphenylene ether and epichlorohydrin. 6.根据权利要求3所述的耐温型多官能团环氧树脂,其特征在于,所述步骤S1-a中,15-冠醚-5催化剂的添加量占双羟基封端聚苯醚和环氧氯丙烷总质量的2~4%。6. The heat-resistant multifunctional epoxy resin according to claim 3, characterized in that, in step S1-a, the amount of 15-crown ether-5 catalyst added accounts for 2-4% of the total mass of dihydroxy-terminated polyphenylene ether and epichlorohydrin. 7.根据权利要求3所述的耐温型多官能团环氧树脂,其特征在于,所述步骤S1-b中,纳滤膜过滤后,滤液需经氧化钙和氧化铝的双金属氧化物脱氯处理。7. The heat-resistant multifunctional epoxy resin according to claim 3, characterized in that, in step S1-b, after nanofiltration, the filtrate needs to be dechlorinated by a bimetallic oxide of calcium oxide and aluminum oxide. 8.根据权利要求1所述的耐温型多官能团环氧树脂,其特征在于,所述环氧改性硅油的制备,包括以下步骤:8. The heat-resistant multifunctional epoxy resin according to claim 1, characterized in that the preparation of the epoxy-modified silicone oil includes the following steps: S2-a、将4-乙烯基苯基缩水甘油醚和氢封端聚二甲基硅氧烷按照不低于2.1:1的摩尔比混合,添加Ashby’s催化剂,配制成反应液;S2-a. Mix 4-vinylphenyl glycidyl ether and hydrogen-terminated polydimethylsiloxane in a molar ratio of not less than 2.1:1, add Ashby’s catalyst, and prepare a reaction solution. S2-b、将步骤S2-a配置的反应液在60~65℃温度下预反应1h以上,而后升温至90~95℃反应4.5h以上,得到反应混合液;S2-b: The reaction solution prepared in step S2-a is pre-reacted at 60~65℃ for more than 1 hour, and then the temperature is raised to 90~95℃ for more than 4.5 hours to obtain a reaction mixture. S2-c、将步骤S2-b得到的反应混合液经活性炭脱色处理,而后过滤滤除活性炭,120~125℃减压蒸馏去除未反应的4-乙烯基苯基缩水甘油醚,制得环氧改性硅油。S2-c: The reaction mixture obtained in step S2-b is decolorized with activated carbon, then filtered to remove the activated carbon, and unreacted 4-vinylphenyl glycidyl ether is removed by vacuum distillation at 120~125℃ to obtain epoxy-modified silicone oil. 9.根据权利要求8所述的耐温型多官能团环氧树脂,其特征在于,所述步骤S2-a中,4-乙烯基苯基缩水甘油醚和氢封端聚二甲基硅氧烷的摩尔比为2.2~2.4:1。9. The heat-resistant multifunctional epoxy resin according to claim 8, characterized in that, in step S2-a, the molar ratio of 4-vinylphenyl glycidyl ether and hydrogen-terminated polydimethylsiloxane is 2.2~2.4:1. 10.一种权利要求1所述的耐温型多官能团环氧树脂的制备方法,其特征在于,包括以下步骤:10. A method for preparing the heat-resistant multifunctional epoxy resin according to claim 1, characterized in that it comprises the following steps: S1、制备环氧封端聚苯醚;S1. Preparation of epoxy-terminated polyphenylene ether; S2、制备环氧改性硅油;S2. Preparation of epoxy-modified silicone oil; S3、按照配比精确称取各组分原料,混合后置于真空干燥箱中,95~105℃固化反应1.5h以上,制得耐温型多官能团环氧树脂。S3. Weigh each component raw material precisely according to the formula, mix them and place them in a vacuum drying oven, cure at 95~105℃ for more than 1.5 hours to obtain a heat-resistant multifunctional epoxy resin.
CN202610096106.9A 2026-01-23 2026-01-23 A temperature-resistant multifunctional epoxy resin and its preparation method Withdrawn CN121574499A (en)