CN122206830A - Method for sealing aluminum alloy using tungsten salt and aluminum-based or aluminum alloy-based component obtained by the method - Google Patents

Method for sealing aluminum alloy using tungsten salt and aluminum-based or aluminum alloy-based component obtained by the method

Info

Publication number
CN122206830A
CN122206830A CN202480073166.8A CN202480073166A CN122206830A CN 122206830 A CN122206830 A CN 122206830A CN 202480073166 A CN202480073166 A CN 202480073166A CN 122206830 A CN122206830 A CN 122206830A
Authority
CN
China
Prior art keywords
aluminium
layer
tungstate
aluminum
aluminum alloy
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN202480073166.8A
Other languages
Chinese (zh)
Inventor
亚历克斯·雅各布尼
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Safran Landing Systems SAS
Original Assignee
Safran Landing Systems SAS
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Safran Landing Systems SAS filed Critical Safran Landing Systems SAS
Publication of CN122206830A publication Critical patent/CN122206830A/en
Pending legal-status Critical Current

Abstract

The invention relates to a component (1) based on aluminium or an aluminium alloy, comprising a body (10) made of aluminium or an aluminium alloy, an inner layer (12) comprising aluminium oxide, an intermediate layer (14) comprising chromium and zirconium, and an outer layer (16) comprising tungsten oxide, which intermediate layer (14) is placed on the body (10), the intermediate layer (12) being placed between the inner layer and the outer layer (16). The invention also relates to a method for post-anodising a body (10) made of aluminium or an aluminium alloy.

Description

Method for sealing aluminum alloy using tungsten salt and aluminum-based or aluminum alloy-based component obtained by the method
Technical Field
The present invention is part of the search for new solutions for corrosion protection of aluminum alloys, in particular for aerospace applications, with or without the application of coating systems.
Background
Aluminum alloys are the material of choice in the transportation industry, particularly in the aerospace industry, due to their excellent mechanical properties/weight ratio and relatively low manufacturing costs. However, depending on the environment in which they are used, these alloys may be affected by several types of localized corrosion, leading to degradation of the component and possibly its removal or failure. A number of strategies have been implemented to overcome this drawback, with the formation or deposition of protective layers on the surface of aluminum alloy components being the most widely used. This is especially true of the protective layer obtained during the anodization process of the aluminum alloy part. Anodization is an electrolytic process that replaces a few nanometers thick native oxide (native oxide) covering aluminum with an oxide layer of up to a few microns. The oxide layer produced by anodization ranges in thickness from 2 microns to about 15 microns to provide long-term corrosion protection. Anodization (also known as anodic oxidation) involves the formation of a porous aluminum oxide/hydroxide layer (known as an anode layer) on the surface of a part that constitutes the anode of an electrolytic system by applying an electrical current to the part immersed in an electrolytic bath containing a strong acid electrolyte. The layer thus formed on the surface of the component can enhance the corrosion resistance of the component after the sealing treatment. Anodizing is now commonly used in the aerospace industry primarily to improve the corrosion resistance of the component, thereby improving the service life of the component, and also to aid in the adhesion of the organic layer (coating). However, the anodising process is directly affected by european Regulations (REACH) which, since month 9 of 2017, prohibit (or limit the use of certain critical elements, in particular hexavalent chromium, in surface treatments. Hexavalent chromium is present in CAA-type anodising (chromic acid anodising, for example as described in www.a3ts.org/actualite/commissions-techniques/fiches-techniques-traitement-surface/anodisation-chromique), but also in usual surface preparation pre-treatments, the purpose of which is to clean/exfoliate the surface of the component prior to anodising and finally in a final treatment, called sealing, the purpose of which is to close the pores of the anode layer formed during anodising.
Different methods have been proposed to replace CAA and SAA (sulfuric acid anodized) treatments using hexavalent chromium seals, which are affected by european regulations REACH:
NGSAA (next generation sulfuric acid anodising, for example as described in "a3ts.org/actualite/commissions-techniques/fiches-techniques-traitement-surface/anodisation-sulfurique-version-5-2") has been proposed to replace SAA;
TSA (tartaric-sulfuric acid anodising, for example as described in "a3ts.org/actualite/commissions-techniques/fiches-techniques-traitement-surface/anodisation-sulfo-tartrique-oast-tartric-sulfuric-anodizing-tsa") has been proposed to replace CAA.
CAA can also be replaced by NGSAA-TL (thin-layer next generation sulfuric acid anodising), NGSAA-TL being anodising of the NGSAA type, the anodising parameters (voltage, immersion time) of which are adjusted to obtain anodising layers with a thickness between 2 μm and 7 μm.
While current conventional anodization solutions, such as NGSAA and subsequent hot water seals, achieve a treatment range compatible with european regulations REACH, they are still unsatisfactory or still unsatisfactory in terms of corrosion protection on certain grades of aluminum alloys known as "difficult". Non-limiting examples of aluminum alloys known as "difficult" include alloys 2214, 2618A or AU5NKZr. These alloys have a specific microstructure due to their chemical composition, which gives them cast defects or precipitates, such as intermetallic compounds rich in copper, iron or nickel. Thus, when an anode layer is formed on the surface of these alloys, layer defects may remain, resulting in some localized brittleness, which is susceptible to corrosion.
Therefore, for these alloys, it is necessary to optimize the range of anodization to improve corrosion resistance.
Patent FR 3106838B1 proposes a method for post-anodising sealing of aluminium or aluminium alloys which improves the corrosion resistance of the component without the use of hexavalent chromium, which is subject to european REACH regulations. The method is also applicable to so-called "difficult" aluminium alloys, which comprises a step of impregnating the aluminium or aluminium alloy in a water bath containing hexafluorozirconate and trivalent chromium salts, followed by a sealing step carried out in an aqueous solution containing alkali or alkaline earth metal silicate, optionally followed by application of a coating. Although improvements in corrosion resistance are brought about by this method, there is a real need to further optimize the current anodizing methods for aluminum or aluminum alloy parts (including so-called "difficult" aluminum alloys) to improve the corrosion resistance of these alloys while meeting the requirements of the european REACH regulations.
The object of the present invention is to remedy the drawbacks of the current methods for anodising components made of aluminium or aluminium alloys, including so-called "difficult" aluminium alloys, in terms of the corrosion resistance properties of said alloys and good paint adhesion.
Furthermore, the present invention aims to provide an aluminium or aluminium alloy component having improved corrosion resistance properties while meeting the requirements of the european REACH regulations.
Disclosure of Invention
The present invention is configured to meet these needs by providing an aluminum or aluminum alloy-based component, characterized in that the component comprises:
A main body made of aluminum or an aluminum alloy,
An inner layer comprising alumina disposed on the body,
An intermediate layer comprising chromium and zirconium, and
An outer layer comprising tungsten oxide, an intermediate layer disposed between the inner and outer layers.
The component may include one or more of the following features:
The component includes a paint layer (18) disposed on the outer layer;
The aluminum alloy is selected from the 2000, 6000 and 7000 series;
the aluminum alloy is an aluminum alloy selected from the group consisting of 2014、2017、2024、2214、2219、2618、AU5NKZr、7175、5052、5086、6061、6063、7010、7020、7050、7050 T7451、7055、7068、7085、7075、7175 and 7475;
The aluminum alloy is a cast aluminum alloy selected from the group consisting of AS7G06, AS7G03, AS10G, and AS9U 3;
The aluminum alloy is a so-called difficult aluminum alloy selected from the group consisting of 2618A, 2214 and AU5 NKZr;
The thickness of the outer layer is between 10 and 500 nm;
the thickness of the paint layer is between 10 and 100 μm.
The invention also relates to a method for post-anodising a body made of aluminium or an aluminium alloy, the method comprising at least the steps of:
A) A step of impregnating anodized aluminum or aluminum alloy in a water bath of demineralized water at a temperature between 20 ℃ and 80 ℃, said water bath containing
Hexafluorozirconate selected from the group consisting of ammonium hexafluorozirconate ((NH 4)2ZrF6), sodium hexafluorozirconate (Na 2ZrF6), potassium hexafluorozirconate (K 2ZrF6), and
A trivalent chromium salt selected from the group consisting of CrF3,xH2O、CrCl3,xH2O、Cr(NO3)3,xH2O、(CH3CO2)2Cr,xH2O、(CH3CO2)7Cr3(OH)2,xH2O、Cr2(SO4)3,xH2O、CrK(SO4)2,xH2O;
B) A sealing step carried out in an aqueous solution containing deionized water having an electrical conductivity of less than or equal to 100 μs/cm, of between 1 and 200g/L, preferably between 5 and 100g/L, of an alkali metal or alkaline earth metal silicate, at a temperature between 60 ℃ and 100 ℃;
c) A post-sealing rinsing step with deionized water having a conductivity of less than or equal to 100 μs/cm and at a temperature between 15 ℃ and 75 ℃.
The method may include one or more of the following features or steps:
In the impregnation step A), the concentration of hexafluorozirconate is between 0.5 and 50 g/L;
in the impregnation step A), the concentration of trivalent chromium salt in this step is between 0.1 and 50 g/L;
The alkali or alkaline earth metal tungstate in step B) is selected from the group consisting of lithium tungstate (Li 2WO4), sodium tungstate (Na 2WO4), potassium tungstate (K 2WO4), calcium tungstate (CaWO 4), zirconium tungstate (Zr (WO 4)2), ammonium tungstate ((NH 4)10H2(W2O7)6);
after step a) and before step B), the method comprises a step of immersing in a bath of lanthanum salt and hydrogen peroxide.
The intermediate flushing, in particular with demineralised water, can be carried out at the following times:
between steps A) and B), and/or
Before and/or after passing through the anodized part.
Since the anodized layer has a very porous structure, it is necessary to seal the anodized layer when chemical resistance and/or corrosion resistance are very important. This means that the aluminum oxide layer is converted into an aluminum hydroxide composite in which the pores are closed. Thus, in addition to anodization, the seal is decisive for the quality of the anodized layer, as:
the sealing of the holes increases corrosion resistance;
Avoiding scaling;
leaching of dye from the pores is avoided.
The post-anodising sealing method of the present invention enables a coating with very high corrosion resistance to be obtained on aluminium alloys known as difficult, such as 2618A and 2214, as well as on aluminium alloys most common in the aeronautical field, such as 2024 or 7175.
The sealing method of the present invention can be applied to various anodization known to those skilled in the art, including CAA (chromic acid anodization), HA (hard anodization), SAA (sulfuric acid anodization), TSA (tartaric acid-sulfuric acid anodization), and NGSAA-TL (thin layer next generation sulfuric acid anodization), NGSAA (next generation sulfuric acid anodization), TSA (tartaric acid-sulfuric acid anodization).
The invention also relates to a method for manufacturing a component based on aluminium or an aluminium alloy according to the invention, comprising at least the following steps:
i) An anodising step of subjecting a body made of aluminium or an aluminium alloy, which may have been previously subjected to a surface preparation step (degreasing, then peeling);
ii) treating the anodized body comprising the inner layer by the post-anodising sealing method according to the invention to obtain in sequence an intermediate layer comprising chromium and zirconium and an outer layer comprising tungsten oxide, and optionally
Iii) A layer of paint is applied.
The invention also relates to a component according to the invention, which may comprise a coating layer, and which is intended for use in the aeronautical field.
Drawings
Further features and advantages of the invention will become apparent from the following detailed description, which is to be understood with reference to the accompanying drawings, in which:
Fig. 1 schematically illustrates the steps of carrying out the post-anodized sealing method of the present invention to surface treat aluminum alloy specimens 2618 T6 and 2024.
FIG. 2 shows the process ranges and operating conditions of the tests performed. SOCOMORE is SOCOCLEAN A3432 is a degreasing agent compatible with aluminum and its alloys. SOCOSURF A1858-a1806 from SOCOMORE is a two-component bath for deoxidizing or bleaching aluminum and its alloys after degreasing or alkaline stripping. SOCOMORE a SOCOSURF TCS bath impregnates the pores of the oxide layer obtained after anodisation of OAS (anodic sulphuric acid oxidation) with Cr (III) and zirconium. Finally, the porous layer was sealed with an aqueous sodium tungstate solution.
Fig. 3 is a schematic cross-sectional view of a component according to one of the embodiments of the invention.
Detailed Description
A first object of the invention relates to a component (1) based on aluminium or an aluminium alloy, characterized in that it comprises:
A body (10) made of aluminum or an aluminum alloy,
An inner layer (12) comprising alumina placed on the body (10),
An intermediate layer (14) comprising chromium and zirconium (Cr III/Zr), and
An outer layer (16) comprising tungsten oxide, the intermediate layer (14) being disposed between the inner layer (12) and the outer layer (16).
As indicated, the component (1) according to the invention comprises a body (10) made of aluminium or an aluminium alloy.
The aluminum alloy may be selected from the 2000, 6000 and 7000 series.
The aluminum alloy may be selected from the group :2014、2017、2024、2214、2219、2618、AU5NKZr、7175、5052、5086、6061、6063、7010、7020、7050、7050 T7451、7055、7068、7085、7075、7175 and 7475 consisting of an aluminum casting alloy selected from the group consisting of AS7G06, AS7G03, AS10G and AS9U3, a so-called difficult aluminum alloy selected from the group consisting of 2618A, 2214 and AU5 NKZr.
The component (1) comprises a body (10) on which an inner layer (12) is placed. The layer (12) comprises alumina. The thickness of the inner layer (12) is between 2 and 30 μm, preferably between 5 and 25 μm. The inner layer (12) is obtained by anodising the body (10) using one of the anodising methods known to those skilled in the art as described above.
The component (1) according to the invention comprises an intermediate layer (14) comprising chromium and zirconium. The thickness of the intermediate layer (14) is between 1 μm and 10 μm, for example between 3 μm and 5 μm. The intermediate layer (14) is obtained at the end of the impregnation step (a) of the body (10) comprising the inner layer (12) under the following conditions.
The component (1) according to the invention further comprises an outer layer (16). An intermediate layer (14) is disposed between the inner layer (12) and the outer layer (16). The outer layer (16) comprises tungsten oxide. The thickness of the outer layer (16) is between 10 and 500nm, preferably 200nm. The outer layer (16) is obtained at the end of a sealing step (B) of the body (10) comprising, in succession, an inner layer (12) and an intermediate layer (14), under the following conditions.
In one embodiment of the invention, the component (1) further comprises a coating layer (18). A paint layer (18) is disposed on the outer layer (16) comprising tungsten oxide. The thickness of the paint layer 18 is between 10 μm and 100 μm, preferably 50 μm. Fig. 3 shows a component (1) according to this embodiment of the invention. If several layers of paint are placed, the total thickness of these layers is between 10 and 100 μm, preferably 50 μm.
The component (1) according to the invention has good corrosion resistance and good paint adhesion. The combination of an intermediate layer (14) comprising chromium and zirconium (Cr III/Zr) with an outer layer (16) comprising tungsten oxide gives the component (1) good corrosion resistance. In addition, the outer layer 16 promotes adhesion of the paint layer (18).
The invention relates to a method for post-anodising a body (10) made of aluminium or an aluminium alloy, comprising at least the following steps:
A) A step of impregnating anodized aluminum or aluminum alloy in a water bath of demineralized water at a temperature between 20 ℃ and 80 ℃, said water bath containing
Hexafluorozirconate selected from the group consisting of ammonium hexafluorozirconate ((NH 4)2ZrF6), sodium hexafluorozirconate (Na 2ZrF6), potassium hexafluorozirconate (K 2ZrF6), and
A trivalent chromium salt selected from the group consisting of CrF3,xH2O、CrCl3,xH2O、Cr(NO3)3,xH2O、(CH3CO2)2Cr,xH2O、(CH3CO2)7Cr3(OH)2,xH2O、Cr2(SO4)3,xH2O、CrK(SO4)2,xH2O;
B) A sealing step carried out in an aqueous solution containing deionized water having an electrical conductivity of less than or equal to 100 μs/cm, of between 1 and 200g/L, preferably between 5 and 100g/L, of an alkali metal or alkaline earth metal silicate, at a temperature between 60 ℃ and 100 ℃;
c) A post-sealing rinsing step with deionized water having a conductivity of less than or equal to 100 μs/cm and at a temperature between 15 ℃ and 75 ℃.
The deposition of tungstate on the CrIII/Zr impregnated anodized surface enhances the corrosion resistance of the aluminum or aluminum alloy component and the adhesion of the coating to the component.
Furthermore, due to their relative hardness, tungstates can affect other properties of aluminum or aluminum alloy components, such as friction, surface hardness, and the like.
As already indicated, the intermediate flushing, in particular with demineralised water, can be carried out at the following times:
between steps A) and B), and/or
Before and/or after passing through the anodized part.
The optimized sealing method of the present invention is applicable to any type of aluminum alloy, including so-called "difficult" alloys, particularly 2000, 6000 and 7000 series aluminum alloys, which have been anodized previously by various methods, including CAA, HA, SAA, TSA, NGSAA-TL, NGSAA, TSA.
Furthermore, the post-anodising sealing method of the present invention is compatible with the requirements associated with the european regulations REACH and gives good corrosion protection on aluminium alloys known as "difficult" (e.g. 2618A, 2214 and AU5 NKZr). The subject method may or may not be followed by the application of a coating.
Thus, the post-anodising sealing method of the present invention is capable of obtaining coatings (outer layers (16)) with very high corrosion resistance on 2000, 6000 and 7000 series aluminium alloys and "difficult" aluminium alloys such as 2618A and 2214, but also on aluminium alloys most commonly used in the aerospace industry such as 2024 and 7175.
In the impregnation step A), the concentration of hexafluorozirconate is between 0.5 and 50 g/L. The concentration of trivalent chromium salt in this step is between 0.1 and 50 g/L.
The trivalent chromium salt may be, for example, one of the commercial products Surtec 650 from SURTEC, lanthane 613.3 from COVENTYA, TCS from SOCOMORE.
In the impregnation step A), the hexafluorozirconate concentration is between 0.5g/L and 50g/L, for example equal to 2g/L.
The temperature of the bath in step a) may be between 20 and 80 ℃. In one embodiment, the temperature of the bath in step a) is between 20 and 60 ℃. According to another embodiment of the invention, the temperature of the bath in step a) is between 35 and 45 ℃.
The pH of the bath in step a) is between 3 and 5, preferably between 3.5 and 4.5, for example between 3.7 and 4.2.
The duration of the immersion in the bath in step a) is between 1 and 40 minutes, preferably between 5 and 30 minutes, for example between 5 and 20 minutes.
After step a) and before step B), the method of the invention may optionally comprise a step of immersing in a bath of lanthanum salt and hydrogen peroxide. This immersing step is well known to those skilled in the art for enhancing the corrosion resistance properties of the body (10).
The alkali or alkaline earth metal tungstate in step B) is selected from the group consisting of lithium tungstate (Li 2WO4), sodium tungstate (Na 2WO4), potassium tungstate (K 2WO4), calcium tungstate (CaWO 4), zirconium tungstate (Zr (WO 4)2), ammonium tungstate ((NH 4)10H2(W2O7)6)).
The alkali or alkaline earth metal tungstate may be, for example, one of the commercial products of lithium tungstate (Li 2WO4), sodium tungstate (Na 2WO4), potassium tungstate (K 2WO4), calcium tungstate (CaWO 4), zirconium tungstate (Zr (WO 4)2), ammonium tungstate ((NH 4)10H2(W2O7)6)), and zirconium tungstate (Zr (WO 4)2) from FISHER SCIENTIFIC, from Sigma-Aldrich brand of Merck.
The sealing in step B) is carried out in an aqueous solution of deionized water having a conductivity of less than or equal to 100. Mu.S/cm, preferably between 1 and 100. Mu.S/cm, for example between 1 and 50. Mu.S/cm.
The concentration of alkali metal or alkaline earth metal silicate in the sealing step B) is preferably between 1 and 50 g/L, for example between 5 and 50 g/L.
In one embodiment of the invention, the temperature of the aqueous solution in step B) is between 80 and 100 ℃. In another embodiment of the invention, the temperature of the aqueous solution in step B) is between 80 and 98 ℃.
The longer the duration of the sealing step B), the more tungstate will be placed. The duration of the sealing step B) is between 1 and 40 minutes, preferably between 5 and 35 minutes, for example between 5 and 30 minutes.
The pH of the sealing solution is less than 12, for example between 7 and 11.5. In one embodiment of the invention, the sealing solution has a pH between 8 and 9.
The sealing is followed by a rinsing step C) carried out in deionized water having a conductivity of less than or equal to 100. Mu.S/cm, preferably between 1 and 100. Mu.S/cm, more preferably between 10 and 100. Mu.S/cm, for example between 10 and 50. Mu.S/cm.
The post-sealing flushing is preferably carried out at a temperature between 10 ℃ and 75 ℃, for example between 15 ℃ and 60 ℃.
The pH of the water in step C) is between 4.5 and 8.5, preferably between 5 and 8, for example between 5.5 and 7.5.
The duration of the flushing after sealing is between 10 seconds and 10 minutes, preferably between 10 seconds and 5 minutes, for example between 30 seconds and 2 minutes.
It has been found, quite unexpectedly, that the combination of the steps of impregnating a) +sealing B) +post-sealing rinsing C) as described below is essential to ensure good corrosion resistance of aluminum or aluminum alloys.
Furthermore, in order to obtain the desired corrosion resistance and properties of the aluminum or aluminum alloy, alkali or alkaline earth metal tungstates must be applied after the impregnation step a).
Intermediate flushing, in particular with demineralised water, can be achieved between the above-mentioned steps.
Before the aluminium or aluminium alloy body (10) is anodized, the body may be subjected to a surface preparation step by degreasing and/or stripping to remove grease, dirt and oxides present on its surface.
The preliminary step of surface preparation may include one or more of the following operations:
Degreasing the solvent to dissolve grease on the surface of the aluminum or aluminum alloy. This may be accomplished by dipping, spraying, or any other method known to those skilled in the art;
Alkaline degreasing to dissolve grease on the surface of aluminum or aluminum alloy. This may be accomplished by dipping, spraying, or any other technique known to those skilled in the art;
Alkaline stripping to naturally dissolve oxides formed on the surface of aluminum or aluminum alloys. This may be accomplished by dipping, spraying, or any other method known to those skilled in the art. At the end of this operation, the aluminum or aluminum alloy is covered with a powdery layer oxidation product of the intermetallic compound, which must be removed by an acid stripping step;
acid stripping to dissolve naturally occurring oxides on the surface of the aluminum or aluminum alloy and/or oxide layers formed on the surface of the part in the alkaline stripping step. This may be accomplished by dipping, spraying, or any other method known to those skilled in the art.
The preliminary step of surface preparation of a body (10) made of aluminium or aluminium alloy to remove grease, dirt and oxides present on the surface of the body by degreasing and/or stripping can be carried out under the conditions described in, for example, application WO 2013/117759.
Intermediate rinsing, in particular with demineralised water, is preferably effected between the above-mentioned successive steps and before passing through the anodised component.
Prior to application of the sealing method of the present invention, a body (10) made of aluminum or an aluminum alloy, which may have been subjected to a surface preparation step of degreasing and/or peeling by one or more of the operations described above, is anodized. Any type of anodization on aluminum known to those skilled in the art may be used.
Various methods have been proposed to replace CAA and SAA (sulfuric acid anodized) treatments using hexavalent chromium seals, which are affected by european REACH regulations:
NGSAA (next generation sulfuric acid anodising, for example as described in "a3ts.org/actualite/commissions-techniques/fiches-techniques-traitement-surface/anodisation-sulfurique-version-5-2") has been proposed to replace SAA;
TSA (tartaric-sulfuric acid anodising, for example as described in "a3ts.org/actualite/commissions-techniques/fiches-techniques-traitement-surface/anodisation-sulfo-tartrique-oast-tartric-sulfuric-anodizing-tsa") has been proposed to replace CAA.
NGSAA-TL thin-layer next generation sulfuric acid anodized, which is a NGSAA anodization method, the anodization parameters (voltage, immersion time) of which have been adjusted to obtain an anodized layer having a thickness of between 2 and 7 μm.
For the purposes of the present invention, TSA, NGSAA-TL and NGSAA anodization methods are preferred.
The surface treatment method of the invention remarkably improves the corrosion resistance of aluminum or aluminum alloy parts and meets the requirements of European REACH regulations.
In addition, the method of the invention provides better conditions for paint adhesion. Furthermore, due to its chemical nature, tungstate may cause surface functionalization, such as an increase in surface hardness or an improvement in friction properties.
The invention also relates to a method for manufacturing a component (1) based on aluminium or an aluminium alloy according to the invention, comprising at least the following steps:
i) -subjecting a body (10) made of aluminium or an aluminium alloy, which may have been previously subjected to a surface preparation step (degreasing, then peeling);
ii) treating the anodized body comprising the inner layer (12) by the post-anodising sealing method according to the invention to obtain in sequence an intermediate layer comprising chromium and zirconium and an outer layer comprising tungsten oxide, and optionally
Iii) A layer of paint (18) is applied.
The invention also relates to a component according to the invention, which may comprise a coating layer, and which is intended for use in the aeronautical field.
Examples
Example 1:
surface treatment method for aluminum alloy parts
Rolled aluminum alloys 2618 T6, 7175 t73 and aluminum alloy 2024 t351 components of 120x60x2mm size machined on one of the two faces were processed according to the following methods.
Firstly, the surface preparation steps of the component are sequentially realized:
Alkaline degreasing by immersing the part in a bath of SOCOCLEAN A3432 (from SOCOMORE) at 11% vol/vol at 45 ℃ for 10 minutes;
flushing with tap water or demineralised water;
Acid stripping by immersing the part in a solution of SOCOSURF% vol/vol A1858-10% vol/vol A1806 (from SOCOMORE) at a temperature of 50 ℃ for 10 minutes;
flushing with tap water or demineralised water.
The peeled and rinsed part is then subjected to an anodising process known to those skilled in the art, during which the part is immersed in a water bath containing sulphuric acid at a concentration of between 160g/L and 220g/L, for example 180 g/L. The bath was run at a temperature of 18 ℃ and maintained at a temperature of 18 ℃. A dc voltage is applied to the immersed component according to a voltage profile that increases from a value of 0V at a rate of 0.4V/min until a voltage value called plateau of 6V is reached. The voltage was held at plateau value for 50 minutes. An anode layer having a thickness of 4 to 7 μm is formed on the surface of the member.
The thickness of the anode layer formed on the component was measured by eddy current according to standard ISO 2360.
The anodized part is then rinsed one or more times, preferably with demineralised water, and then subjected to the impregnation and sealing operations according to the invention under the following conditions and sequences:
Step A) the step of impregnating the part, sequentially impregnating the part in a water bath of SOCOSURF TCS (from SOCOMORE) at a temperature of 40℃and a pH of 3.9 for 10 minutes and in a water bath of SOCOSURF PACS (from SOCOMORE) at a temperature of 25℃and a pH of between 4.5 and 5.5 for 5 minutes at 34% vol/vol, then
Step B) sealing by immersing the part at the end of the impregnation step A) in 20g/L sodium tungstate aqueous solution at a temperature of 98℃and a pH of less than 12, for example a pH of 8 to 9, for 10 minutes, then
Step C) post-sealing rinse by immersing these operated parts in deionized water having a conductivity of less than 100 μS/cm for 1 minute at a temperature of 20 ℃.
Between each step, a rinse is performed with demineralised water.
Corrosion resistance results evaluated for anodized alloys sealed by conventional sealing methods and by the sealing methods of the invention:
by way of comparison, aluminum alloy parts anodized using the methods shown above were subjected to sealing operations, such as hydrothermal sealing (CrIII/Zr+ water) and silicate sealing (CrIII/Zr+ silicate), using methods known to those skilled in the art (WO 2021/152241 for silicate sealing), and compared to parts sealed using the methods of the invention (CrIII/Zr+ sodium tungstate). The parts treated in this way were subjected to the salt spray test (BS) according to standard NF EN ISO 9227. The pit numbers after 500 hours of salt mist (BS) are shown in table 1 below.
TABLE 1
From the results two conclusions can be drawn:
1-comparing the configuration of reference 2 with other configurations, it is apparent that the tungstate and silicate seals improved the corrosion resistance of the anodized layer in terms of the number of pits per specimen.
2-Reference 1 will be compared to the tungstate configuration, the corrosion resistance of the tungstate seal anodized was comparable to the corrosion resistance of the silicate seal layer in terms of the number of pits per coupon.
Thus, the tungstate-based seals according to the invention after anodisation achieve better corrosion resistance than the hydrothermal seals and are comparable to the silicate-based seals described in WO 2021/152241.
Extreme surface analysis (XPS and EDX)
X-ray photoelectron spectroscopy (XPS) was performed on a Thermo K-alpha+ instrument with monochromatic Al Kalpha source processing software, advantage.
The following sample surfaces were subjected to X-ray photoelectron spectroscopy (XPS) analysis:
the surface of the sample (referred to as 109-NaW in Table 2 below) that had been seal anodized with CrIII/Zr+tungstate;
the surface of a sample (referred to as 110-HWS in the following table) that has been seal anodized with CrIII/Zr+H 2 O;
So as to have a reference for the presence of tungstate on the surface, as compared to another type of seal.
TABLE 2
Al (III) and Cr (III) refer to these elements as oxides or hydroxides.
Enrichment of tungsten in oxidized form (presence of oxygen) was detected as shown by elemental analysis of the extreme surface (50 nm surface) w=7.19 and o=74.47. This confirms the presence of silicate on the surface.
The deposition of tungstate on the Cr (III)/Zr impregnated anodized surface improves the corrosion resistance of the chromium-free anodized.
Paint adhesion test
The parts treated by the sealing method according to the invention were subjected to a paint adhesion test. The painted parts were characterized after immersion in various aggressive liquids (water, skydrol). Adhesion rating for such tests ranges from 0 (no degradation) to 5 (complete degradation) according to ISO 2409
Overall results indicate that the coating passing the tungstate seal test has very good adhesion.

Claims (11)

1. A component (1) based on aluminium or an aluminium alloy, characterized in that it comprises:
A body (10) made of aluminum or an aluminum alloy,
An inner layer (12) comprising alumina placed on said body (10),
An intermediate layer (14) comprising chromium and zirconium, and
An outer layer (16) comprising tungsten oxide, the intermediate layer (14) being disposed between the inner layer (12) and the outer layer (16).
2. The component according to claim 1, characterized in that it comprises a paint layer (18) placed on the outer layer (16).
3. The component according to claim 1 or 2, wherein the aluminum alloy is:
An aluminum alloy selected from the group consisting of 2014、2017、2024、2214、2219、2618、AU5NKZr、7175、5052、5086、6061、6063、7010、7020、7050、7050 T7451、7055、7068、7085、7075、7175 and 7475, or
Cast aluminum alloy selected from the group consisting of AS7G06, AS7G03, AS10G and AS9U3, or
So-called difficult aluminum alloys selected from the group consisting of 2618A, 2214 and AU5 NKZr.
4. A component according to any one of claims 1 to 3, characterized in that the thickness of the outer layer (16) is between 10 and 500 nm.
5. A component according to any one of claims 2 and 3, characterized in that the thickness of the coating layer (18) is between 10 and 100 μm.
6. A method for post-anodising a body (10) made of aluminium or an aluminium alloy, the method comprising at least the steps of:
A) A step of impregnating the anodized body (10) made of aluminium or an aluminium alloy in a water bath of demineralised water at a temperature between 20 ℃ and 80 ℃, said body comprising an inner layer (12) comprising aluminium oxide, said water bath containing
Hexafluorozirconate selected from the group consisting of ammonium hexafluorozirconate ((NH 4)2ZrF6), sodium hexafluorozirconate (Na 2ZrF6), potassium hexafluorozirconate (K 2ZrF6), and
A trivalent chromium salt selected from the group consisting of CrF3,xH2O、CrCl3,xH2O、Cr(NO3)3,xH2O、(CH3CO2)2Cr,xH2O、(CH3CO2)7Cr3(OH)2,xH2O、Cr2(SO4)3,xH2O、CrK(SO4)2,xH2O;
B) A sealing step carried out in an aqueous solution containing between 1 and 100g/L of deionized water having a conductivity of less than or equal to 100 μs/cm at a temperature between 60 ℃ and 100 ℃;
c) A post-sealing rinsing step with deionized water having a conductivity of less than or equal to 100 μs/cm and at a temperature between 15 ℃ and 75 ℃.
7. The process according to claim 6, wherein in the impregnation step A) the hexafluorozirconate concentration is between 0.5 and 50 g/L.
8. The method according to claim 6 or 7, characterized in that in the impregnation step a) the concentration of trivalent chromium salt in this step is between 0.1 and 50g/L.
9. The method according to any one of claims 6 to 8, wherein the alkali or alkaline earth metal tungstate in step B) is selected from the group consisting of lithium tungstate (Li 2WO4), sodium tungstate (Na 2WO4), potassium tungstate (K 2WO4), calcium tungstate (CaWO 4), zirconium tungstate (Zr (WO 4)2), ammonium tungstate ((NH 4)10H2(W2O7)6).
10. The method according to any one of claims 6 to 9, characterized in that it comprises, after step a) and before step B), a step immersed in a bath of lanthanum salt and hydrogen peroxide.
11. Method for manufacturing an aluminium or aluminium alloy based component (1) according to any one of claims 1 to 5, the method comprising at least the steps of:
i) -subjecting a body (10) made of aluminium or an aluminium alloy, which may have been previously subjected to a surface preparation step (degreasing, then peeling);
ii) treating the anodized body comprising an inner layer (12) by the post-anodising sealing method according to any one of claims 6 to 9 to obtain in sequence an intermediate layer (14) comprising chromium and zirconium and an outer layer (16) comprising tungsten oxide, and optionally
Iii) A layer of paint (18) is applied.
CN202480073166.8A 2023-11-16 2024-11-12 Method for sealing aluminum alloy using tungsten salt and aluminum-based or aluminum alloy-based component obtained by the method Pending CN122206830A (en)