Disclosure of Invention
The invention aims to overcome the defects of easy instability, low dimensional accuracy and insufficient production efficiency in the existing thick-wall cylinder hydraulic bulging process, and provides the hydraulic bulging process for controlling the instability of the thick-wall cylinder, so that uniform deformation of the thick-wall cylinder bulging process is realized, instability phenomena such as bulging, waist concave, bell mouth and the like are effectively inhibited, the dimensional accuracy and the product qualification rate of formed parts are improved, simultaneously, the real-time monitoring and active regulation of the instability are realized, and the production efficiency is improved.
The invention is realized by the following technical scheme:
A hydro-bulging process for destabilization control of thick-walled cylinders comprising the steps of:
S1, blank pretreatment, which comprises the following steps of firstly detecting the initial overall dimension, microscopic grain size and grain size uniformity of a blank, secondly removing oxide skin, burrs and scratches on the surface of the blank to ensure the surface of the blank to be clean and smooth, thirdly carrying out ultrasonic flaw detection on the blank to ensure that no obvious defects exist in the blank, ensuring the mechanical properties of the blank to be uniform, and avoiding instability caused by defect expansion in the bulging process, and finally, machining C10 chamfers (10 mm multiplied by 45 DEG chamfers) at the upper and lower inner circular ports of the blank to facilitate the lamination and sealing with a special force-reducing hydraulic bulging die punch in the hydraulic bulging process;
S2, determining a judgment basis of blank hydro-bulging instability, which comprises the following steps:
Firstly, a metal mechanical property test is carried out, namely a standard tensile sample is prepared by selecting a sample which is the same as a blank and is in the same heat treatment state, the standard tensile sample is adopted for carrying out the tensile test, the mechanical property parameters of the material are obtained, the mechanical behavior of the material in the cold deformation process under the room temperature condition is represented, and accurate parameter support is provided for the subsequent establishment of a hydraulic bulging process and simulation modeling;
Then, drawing a real stress-strain curve of the material according to mechanical property parameters of the material, and fitting the real stress-strain curve in Origin software by adopting a nonlinear power exponent hardening model sigma true=Kεtrue m, wherein K is a hardening coefficient, epsilon true is a hydraulic bulging deformation amount, and m is a strengthening coefficient;
Finally, determining the judgment basis of material hydro-expansion instability (tangential necking) according to the hydro-expansion deformation epsilon (determined according to the bulging strengthening technical requirement), wherein the judgment basis is epsilon true is less than or equal to 2m, if epsilon true is less than or equal to 2m, the blank is considered to be difficult to generate hydro-expansion instability in the subsequent hydro-expansion process, the blank meets the requirement of the subsequent hydro-expansion, if epsilon true is more than 2m, the blank is easy to generate hydro-expansion instability in the subsequent hydro-expansion process, and the value of the strengthening coefficient m of the material needs to be increased until epsilon true is less than or equal to 2m;
S3, performing flow-solid coupling CEL analysis (Coupled Eulerian-Lagrangian is a mainstream numerical method specially solving the problems of large deformation, strong impact and free liquid surface flow-solid coupling) by adopting ABAQUS finite element simulation software, wherein the core is that solid and Euler grid computing fluids are computed by using Lagrangian grids, and bidirectional interaction is realized through interface coupling), a thick-wall cylinder hydraulic bulging finite element model is established, an actual hydraulic bulging working condition is simulated, technological parameters are optimized and adjusted, and the optimal loading rate is determined;
S4, die assembly and blank installation;
S5, hydraulic bulging is carried out by adopting a two-section loading mode according to the optimized technological parameters in the step S3, and the method comprises the following steps:
S5-1, in an initial bulging stage, the pressure in a hydraulic medium is rapidly increased from 0 to 130-150 MPa, the loading rate of an upper punch is 10-20 mm/S, and the core of the stage is that an bulging device rapidly builds ultrahigh pressure so that a blank is rapidly and uniformly stressed and enters a plastic deformation state. The problem that partial hydraulic medium is not continuously sprayed due to too slow pressure rising in the initial stage, so that the hydraulic pressure is unstable, the blank is subjected to uneven internal pressure, and the shape instability is induced is avoided;
S5-2, in a stable bulging stage, the loading rate of an upper punch is kept 15-20 mm/S, the internal pressure is continuously pressurized to 150-300 MPa, the process hardening characteristic of a material is utilized, the bulging internal pressure of a thick-wall cylinder is uniform and stable through stable loading speed control, the strength of the material is gradually improved, local deformation is restrained from being overlarge, shape instability is avoided, the requirement of dimensional accuracy is met, the outline dimension data of a blank in the stable bulging stage are monitored in real time through a visual displacement sensor, if the blank is found to have a bulge, a concave waist or a horn shape instability phenomenon, the bulging process is immediately stopped, the outline dimension of the blank is unloaded and accurately measured, the loading rate of the upper punch is adjusted according to the outline shape and dimension measurement result of the blank, then the blank is reloaded on a force-reducing hydraulic bulging die, the blank is continuously bulging, and the processing method after the instability phenomenon is generated is specifically as follows:
a) Firstly, determining that the deflection of an outer bus of the blank is delta mm, if delta mm is less than 7mm, carrying out subsequent steps, if delta mm is more than or equal to 7mm, stopping bulging processing of the blank, and then reducing the value of the loading rate of an upper punch by 1-2 times of the deflection value delta;
b) Firstly, determining that the deflection of an outer bus of the blank is delta mm, if delta mm is less than 7mm, carrying out subsequent steps, if delta mm is more than or equal to 7mm, stopping bulging processing of the blank, then increasing the value of the loading rate of an upper punch by 1-2 times of the deflection value delta, repeating the step b) if the concave waist shape still appears in the bulging process of the blank after the loading rate of the upper punch is increased, increasing the loading rate of the upper punch until the outer bus of the blank is flat, and if the loading rate of the upper punch reaches the maximum limit value or the whole blank is still concave waist shape after the bulging of the upper punch is increased, increasing the chamfer of 5-10 mm on the basis of the chamfer of the upper inner circle port and the lower inner circle port of the blank;
c) The method comprises the steps of respectively measuring the outer diameters of a large end and a small end at the bell mouth position of a blank, calculating the ratio of the outer diameter of the large end to the outer diameter of the small end to be c, increasing the chamfer angle of the inner round port of the blank corresponding to the small end to be 5 degrees if c is more than or equal to 0.98, increasing the chamfer angle of the inner round port of the blank corresponding to the small end to be 10 degrees if c is more than or equal to 0.96 and less than or equal to 0.98, increasing the chamfer angle of the inner round port of the blank corresponding to the small end to be 15 degrees if c is more than or equal to 0.94 and increasing the chamfer angle of the inner round port of the blank corresponding to the small end to be 20 degrees if c is less than or equal to 0.94;
d) If the blank is expanded and then the whole body is in a mixed shape and unstable, if the blank is expanded and then the whole body is in a horn mouth shape and is accompanied by the instability of a drum belly shape, the loading rate of the upper punch and the chamfering angle of the inner circular port of the blank are adjusted according to the steps a) and c) until the outer bus of the blank is flat, and if the blank is expanded and then the whole body is in a horn mouth shape and is accompanied by the instability of a concave waist shape, the loading rate of the upper punch and the chamfering angle of the inner circular port of the blank are adjusted according to the steps b) and c) until the outer bus of the blank is flat.
S5-3, unloading, namely when the pressure equipment reaches a preset stroke, the blank is swelled to a calibrated size, the pressure equipment beam is lifted up rapidly, pressure is relieved rapidly, instability phenomenon caused by unstable internal pressure due to discontinuous spraying of the hydraulic medium or uneven local leakage of the liquid is avoided, and hydraulic bulging of the blank is completed, so that the hydraulic bulging thick-wall cylinder is manufactured.
Further, in the step S2, the mechanical property parameters include yield strength, tensile strength, uniform elongation, total elongation, elastic modulus, poisson' S ratio, hardening coefficient, and strengthening coefficient.
Further, the step S3 includes the steps of:
Firstly, a thick-wall cylinder hydraulic bulging geometric model is established in ABAQUS finite element simulation software and grids are divided, wherein the geometric model comprises a blank, a hydraulic medium, an upper punch, a lower punch and a force reducing column of a force reducing hydraulic bulging die;
secondly, inputting the mechanical property parameters of the material obtained in the step S2 into a simulation model to serve as core parameters of a constitutive relation of the material, ensuring that the model can truly reflect the mechanical response of the material, and setting a hydraulic medium as water;
Thirdly, setting a plastic flow criterion of the material according to the real stress-strain curve determined in the step S2, setting a friction coefficient between a die and a blank and loading boundary constraint, and simulating a contact state and constraint conditions in an actual bulging process;
finally, the relation among the loading rate of the pressure equipment, the spraying volume of the hydraulic medium and the cylindrical shape size of the thick wall is analyzed by simulating bulging processes under different loading rates of the upper punch, the process parameters are optimally adjusted, the optimal loading rate is determined, and the blank is ensured not to be unstable such as bulging, loudspeaker and the like.
Further, in the step S5, if the hydro-bulging deformation amount epsilon true is greater than 0.2 or the hydraulic press forming force F < P maxπ(r2-r Reduction of 2),Pmax is the maximum internal pressure of the liquid, r is the inner diameter of the blank, r Reduction of is the radius of the force-reducing column, the diameter of the force-reducing column is increased, and the steps S4 and S5 are repeated until the preset size is reached.
Further, detecting the diameter, the wall thickness and the roundness of the hydraulic bulging thick-wall cylinder by adopting a detecting instrument, adjusting unqualified parts according to the instability phenomenon, and then bulging again until the product is qualified in detection.
The invention has the beneficial effects that:
1. According to the invention, through a preliminary metal mechanical property test, the mechanical behavior of the material is comprehensively represented, and the plasticity and the strengthening characteristic of the material are analyzed by combining the stress-strain curve, so that the expansion necking instability caused by insufficient material performance is avoided in advance, and a foundation is provided for the implementation of the subsequent expansion process;
2. According to the invention, by combining a finite element simulation technology, the mechanical behavior parameters of the material are accurately set, the shape change rule and stress strain distribution of a thick-wall cylinder blank in the bulging process are simulated, the instability risk point is predicted, the blindness of optimizing process formulation in the prior art is solved, the accurate prediction and control of the bulging instability of the thick-wall cylinder are realized, the instability defects such as bulging belly, concave waist, bell mouth and the like are effectively inhibited, and the scientificity and rationality of the process are improved from the source;
3. The invention adopts a strategy of accurately controlling the loading speed of the pressure equipment and the size of the blank to implement measurement and control, realizes quick pressurization and quick unloading, ensures quick response and continuous and uniform establishment of high pressure in the bulging of the thick-wall cylinder, and avoids the instability problem caused by uneven stress of the blank. Meanwhile, the invention also provides a specific adjustment solution for the abnormal instability of bulging, concave waist, bell mouth and the like of the thick-wall cylinder blank, so that the dimensional accuracy and the forming quality of the product are improved, and the qualification rate of the product is improved to more than 98%;
4. The invention is designed for the manganese-chromium austenitic stainless steel thick-wall cylinder forgings such as the nonmagnetic retaining ring of the 50 MW-1000 MW steam turbine generator, has strong adaptability, solves the technical bottlenecks of large bulging difficulty and difficult control of instability of the forgings, reduces the production cost, and has important engineering application value for localization of the booster thick-wall cylinder forgings.
5. The invention defines the association logic of metal mechanical property test, stress-strain curve analysis and finite element simulation parameter setting, forms a complete technology system of test-simulation-process optimization, and provides a borrowable technical scheme for hydraulic bulging processing of similar thick-wall cylinder forgings.
Detailed Description
The invention is described in further detail below with reference to the drawings and examples.
Example 1
In the embodiment 1, a Mn18Cr18N high-nitrogen austenitic stainless steel thick-wall cylinder is selected as a blank for processing a non-magnetic retaining ring of a 300MW steam turbine generator, the dimension requirement after the retaining ring is expanded is 1210 mm, 990 mm is an inner diameter, 110 mm is a wall thickness, the height is 910 mm, and the requirement of an initial blank meets the hot forging technical requirement of the non-magnetic retaining ring of the 50 MW-1000 MW steam turbine generator;
a hydro-bulging process for the destabilization control of thick-walled cylinders as shown in fig. 1 comprising the steps of:
S1, preprocessing a blank, wherein the method comprises the following steps of:
firstly, detecting the initial external dimension, microscopic grain size and grain size uniformity of a blank, selecting a Mn18Cr18N thick-wall cylinder blank, wherein the external diameter is 937 mm, the internal diameter is 672 mm, the wall thickness is 132.5 mm, and the height is 1034 mm;
Secondly, removing oxide skin, burrs and scratches on the surface of the blank, and ensuring the surface of the blank to be clean and smooth;
thirdly, carrying out ultrasonic flaw detection on the blank, ensuring that no obvious defect exists in the blank, and ensuring that the mechanical properties of the blank are uniform;
finally, machining C10 chamfers on the upper and lower inner circular ports of the blank.
S2, determining a judgment basis of blank hydro-bulging instability, which comprises the following steps:
Firstly, a standard tensile sample is prepared by selecting a sample which is the same as a blank and is in the same heat treatment state, axial tension is applied by a WDW3200 micro-control electronic universal tester, the standard tensile sample is adopted for tensile test (the standard tensile sample is prepared according to GB/T228-2002 ' room temperature tensile test method for metallic materials ', the axial tension is applied by the electronic universal tester, load and elongation data are synchronously recorded until the standard tensile sample breaks), and the mechanical performance parameters of the material are obtained, namely, the yield strength is 640 MPa, the tensile strength is 970 MPa, the uniform elongation is 42%, the total elongation is 58%, the elastic modulus is 200 GPa and the Poisson's ratio is 0.3;
Then, drawing a real stress-strain curve of the material according to mechanical property parameters of the material, fitting the real stress-strain curve in Origin software by adopting a nonlinear power exponent hardening model sigma true=Kεtrue m, wherein a hardening coefficient K=1445, a hydraulic bulging deformation epsilon true =0.307, and determining a strengthening coefficient m=0.216 of the material;
Finally, epsilon true =0.307 and m=0.216 are substituted into the material instability judging basis to know epsilon true is less than or equal to 2m, so that the blank provided in the embodiment 1 is not easy to generate hydro-bulging instability in the subsequent hydro-bulging process, and the blank meets the requirement of the subsequent hydro-bulging, namely the bulging does not generate tangential necking instability, the material plasticity is good, the work hardening characteristic is obvious, and the method is suitable for the hydro-bulging processing.
S3, finite element simulation modeling and parameter setting, namely performing flow-solid coupling CEL analysis by adopting ABAQUS finite element simulation software, establishing a thick-wall cylinder hydraulic bulging finite element model, simulating actual hydraulic bulging working conditions, optimizing and adjusting process parameters, and determining optimal loading rate, wherein the method comprises the following steps:
firstly, establishing a thick-wall cylinder hydraulic bulging geometric model in ABAQUS finite element simulation software and dividing grids, wherein the geometric model comprises a blank, a hydraulic medium, an upper punch, a lower punch and a force reducing column of a force reducing hydraulic bulging die;
secondly, inputting mechanical property parameters of the material obtained in the step S2 into a simulation model, and setting a hydraulic medium as water;
Thirdly, setting a plastic flow criterion of the material according to the real stress-strain curve determined in the step S2, selecting Mi Saisi yield criterion in the embodiment 1, matching the plastic deformation rule of Mn18Cr18N steel in a complex stress state, accurately predicting the yield and plastic deformation process of the material, setting the friction coefficient between the die and the blank to be 0.1, loading boundary constraint, and simulating the contact state and constraint condition in the actual bulging process;
Finally, the relationship among the loading rate of the pressure equipment, the spraying volume of the hydraulic medium and the cylindrical shape size of the thick wall is analyzed by simulating bulging processes under different loading rates of the upper punch, the process parameters are optimized and adjusted, and the optimal loading rate is determined.
S4, die assembly and blank installation;
Firstly, checking forming force based on the tonnage of the press and the size of a die, and ensuring that the tonnage of the press meets enough forming force. And selecting an 8000 ton press, selecting two sets of special force-reducing hydraulic bulging dies for double-pass forming, wherein the diameters of force-reducing columns are 650 mm and 800 mm respectively, calculating forming passes, and preparing the special force-reducing hydraulic bulging dies with corresponding sets. Checking the working size of the die, assembling and measuring, cleaning the moving part, ensuring flexible action, repairing damaged parts and ensuring good working state of the die. Preparing tooling auxiliary tools such as measuring tools, sealing rings, lifting tools, butter, cotton yarns, protective covers and the like;
Then cleaning the working walking table of the hydraulic press, horizontally placing the lower die of the force-reducing hydraulic bulging die in the center of the walking table, uniformly smearing butter on the chamfer positions of the upper and lower ends of the blank, the working conical surface of the die and the surface of the guide post, lifting the ring blank by using a binding belt, centering and sleeving the ring blank on the guide post, leveling, lifting the upper punch and the spherical cushion together and stably lifting the ring blank sleeved on the guide post, slightly lifting after centering, filling tap water into a gap, ensuring that the water is full and not leaked, pressing the ring blank by falling, installing a visual displacement sensor to detect the real-time dimension of the blank in the hydraulic bulging process, stably conveying the bulging die and the ring blank under the movable hydraulic press beam, and measuring and recording the initial flange spacing of the upper punch and the lower punch of the die before bulging. The work is ready and then ready for compression bulging.
S5, hydraulic bulging, which comprises the following steps:
S5-1, in an initial bulging stage, rapidly loading, wherein the pressure in a hydraulic medium is rapidly increased from 0 to 150MPa, and the loading rate of an upper punch is 12mm/S;
S5-2, in the stable bulging stage, the loading speed of the upper punch is kept at 15mm/S, the internal pressure is continuously pressurized to 271MPa, and in the embodiment 1, when the stroke of the press reaches 223mm, the blank size in the stable bulging stage is monitored in real time through a visual displacement sensor, and the blank is found to have the instability phenomenon of the concave waist shape. The pressure equipment beam is lifted up quickly, the pressure is relieved quickly, and bulging is stopped. And measuring the size of the blank, wherein the blank is slightly concave, the busbar deflection delta is 3mm, and the loading rate of the upper punch is increased by 1-2 times of the deflection value delta, namely the loading rate of the upper punch is increased to 18mm/s, and bulging is performed again. Correspondingly, if the whole blank is unstable in the shape of a bulge after bulging, the value of the loading rate of the upper punch is reduced by 1-2 times of the deflection value delta, namely, if the slight bulge appears in the stable bulging stage of the blank and the busbar deflection delta is 3mm, the loading rate of the upper punch is reduced to 9-12 mm/s, and bulging is performed again. In this example 1, when the press stroke reaches 348mm, the grommet expands a first time to the nominal size, the pressure equipment beam lifts up rapidly, and pressure is relieved rapidly. In the hydraulic bulging process, blank size data are monitored in real time through a visual displacement sensor, and the phenomena of shape instability such as bulging, concave waist or loudspeaker are avoided. After unloading, measuring the sizes of blanks, wherein the sizes of the blanks are 1115mm in outer diameter, 882.4mm in inner diameter and 948mm in height, and the bus is straight;
And replacing the hydraulic bulging die with the diameter of the force reducing column of 800mm to perform second-pass bulging. The die mounting repeats the above step S4. During hydraulic bulging, the initial bulging stage is quickly loaded, the pressure in a hydraulic medium is quickly increased from 0 to 150MPa, the loading speed of an upper punch is controlled to be 15mm/s, the loading speed of the upper punch is stabilized at 18mm/s as much as possible in the stable bulging stage, and the pressure is gradually increased to 282MPa. When the stroke of the press reaches 232mm, the guard ring is expanded to the calibrated size in the second pass, and the pressure equipment beam is quickly lifted and quickly relieved. The blank size data is monitored in real time through a visual displacement sensor, so that the instability phenomenon does not occur;
S5-3, unloading, namely expanding the blank to a calibrated size when the pressure equipment reaches a preset stroke, rapidly lifting the pressure equipment beam, rapidly releasing pressure, and completing hydraulic expansion of the blank to obtain the hydraulic expansion thick-wall cylinder. And after unloading, measuring the size of the blank, wherein a blank bus is straight and reaches a preset size, specifically, the outer diameter is 1210mm, the inner diameter is 990mm, the wall thickness is 110mm, the height is 910mm, and the hydraulic bulging is finished.
On the basis, a detecting instrument is adopted to detect the diameter, the wall thickness and the roundness of the hydraulic bulging thick-wall cylinder, unqualified parts are adjusted according to the instability phenomenon, then bulging is carried out again until the product is detected to be qualified, the product enters a subsequent processing procedure, and finally the thick-wall cylinder forge piece such as the nonmagnetic retaining ring of the 50 MW-1000 MW steam turbine generator meeting the requirements is obtained.
Example 2
In the embodiment 2, a Mn18Cr18N high-nitrogen austenitic stainless steel thick-wall cylinder is selected as a blank, and is used for processing a non-magnetic retaining ring of a 1000MW steam turbine generator, the size requirement after the retaining ring is expanded is 2060 mm, the inner diameter 1830 mm, the wall thickness is 115mm, the height is 1016mm, and the requirement of an initial blank meets the hot forging technical requirement of the non-magnetic retaining ring of the 1000MW steam turbine generator;
a hydro-bulging process for the destabilization control of thick-walled cylinders as shown in fig. 1 comprising the steps of:
S1, preprocessing a blank, wherein the method comprises the following steps of:
Firstly, detecting the initial external dimension, microscopic grain size and grain size uniformity of a blank, selecting a Mn18Cr18N thick-wall cylinder blank with the outer diameter of 1700mm, the inner diameter of 1450mm, the wall thickness of 125mm and the height of 1120mm;
Secondly, removing oxide skin, burrs and scratches on the surface of the blank, and ensuring the surface of the blank to be clean and smooth;
thirdly, carrying out ultrasonic flaw detection on the blank, ensuring that no obvious defect exists in the blank, and ensuring that the mechanical properties of the blank are uniform;
finally, machining C10 chamfers on the upper and lower inner circular ports of the blank.
S2, determining a judgment basis of blank hydro-bulging instability, which comprises the following steps:
Firstly, a standard tensile sample is prepared by selecting a sample which is the same as a blank and is in the same heat treatment state, axial tension is applied by a WDW3200 micro-control electronic universal tester, the standard tensile sample is adopted for tensile test (the standard tensile sample is prepared according to GB/T228-2002 ' room temperature tensile test method for metallic materials ', the axial tension is applied by the electronic universal tester, load and elongation data are synchronously recorded until the standard tensile sample breaks), and the mechanical performance parameters of the material are obtained, namely, the yield strength is 600 MPa, the tensile strength is 980 MPa, the uniform elongation is 38%, the total elongation is 51%, the elastic modulus is 200GPa, and the Poisson's ratio is 0.3;
then, drawing a real stress-strain curve of the material according to mechanical property parameters of the material, fitting the real stress-strain curve in Origin software by adopting a nonlinear power exponent hardening model sigma true=Kεtrue m, wherein a hardening coefficient K=1402 and a hydro-bulging deformation epsilon true =0.201, and determining a strengthening coefficient m=0.202 of the material;
Finally, epsilon true =0.201 and m=0.202 are substituted into the material instability judging basis to know epsilon true is less than or equal to 2m, so that the blank provided in the embodiment 2 is not easy to generate hydro-bulging instability in the subsequent hydro-bulging process, the blank meets the requirement of the subsequent hydro-bulging, namely the bulging does not generate tangential necking instability, the material plasticity is good, the work hardening characteristic is obvious, and the method is suitable for the hydro-bulging processing.
S3, finite element simulation modeling and parameter setting, namely performing flow-solid coupling CEL analysis by adopting ABAQUS finite element simulation software, establishing a thick-wall cylinder hydraulic bulging finite element model, simulating actual hydraulic bulging working conditions, optimizing and adjusting process parameters, and determining optimal loading rate, wherein the method comprises the following steps:
firstly, establishing a thick-wall cylinder hydraulic bulging geometric model in ABAQUS finite element simulation software and dividing grids, wherein the geometric model comprises a blank, a hydraulic medium, an upper punch, a lower punch and a force reducing column of a force reducing hydraulic bulging die;
secondly, inputting mechanical property parameters of the material obtained in the step S2 into a simulation model, and setting a hydraulic medium as water;
Thirdly, setting a plastic flow criterion of the material according to the real stress-strain curve determined in the step S2, selecting Mi Saisi yield criterion in the embodiment 2, matching the plastic deformation rule of Mn18Cr18N steel in a complex stress state, accurately predicting the yield and plastic deformation process of the material, setting the friction coefficient between the die and the blank to be 0.1, loading boundary constraint, and simulating the contact state and constraint condition in the actual bulging process;
Finally, the relationship among the loading rate of the pressure equipment, the spraying volume of the hydraulic medium and the cylindrical shape size of the thick wall is analyzed by simulating bulging processes under different loading rates of the upper punch, the process parameters are optimized and adjusted, and the optimal loading rate is determined. The method is characterized in that the speed of the initial bulging stage is 14 mm/s, the speed of the stable stage is 18 mm/s, the internal pressure is 165 and MPa of the maximum hydraulic pressure of the first pass, and 178 and MPa of the maximum hydraulic pressure of the second pass, so that the thick-wall cylinder blank is ensured not to be unstable such as bulging, loudspeaker and the like.
S4, die assembly and blank installation;
Firstly, checking forming force based on the tonnage of the press and the size of a die, and ensuring that the tonnage of the press meets enough forming force. Selecting 18500 ton press, selecting two sets of special force-reducing hydraulic bulging dies for double-pass forming, wherein the diameters of force-reducing columns are 1130 mm and 1300 mm respectively, calculating forming passes, and preparing the special force-reducing hydraulic bulging dies with corresponding sets. Checking the working size of the die, assembling and measuring, cleaning the moving part, ensuring flexible action, repairing damaged parts and ensuring good working state of the die. Preparing tooling auxiliary tools such as measuring tools, sealing rings, lifting tools, butter, cotton yarns, protective covers and the like;
Then cleaning the working walking table of the hydraulic press, horizontally placing the lower die of the force-reducing hydraulic bulging die in the center of the walking table, uniformly smearing butter on the chamfer positions of the upper and lower ends of the blank and the working conical surfaces of the die and the surfaces of the guide posts, lifting the ring blank by using a binding belt, centering and leveling, lifting the upper punch and the spherical pad together and stably lifting the ring blank sleeved on the guide posts, slightly lifting the ring blank after centering, filling tap water into a gap to ensure that the water is full, pressing the ring blank by falling, installing a visual displacement sensor to detect the real-time dimension of the blank in the hydraulic bulging process, stably conveying the bulging die and the ring blank under the movable hydraulic press beam, and measuring and recording the initial flange spacing of the upper punch and the lower punch of the die before bulging. The work is ready and then ready for compression bulging.
S5, hydraulic bulging, which comprises the following steps:
s5-1, in an initial bulging stage, rapidly loading, wherein the pressure in a hydraulic medium is rapidly increased from 0 to 150MPa, and the loading rate of an upper punch is 14mm/S;
s5-2, in a stable bulging stage, the loading speed of the upper punch is kept at 18mm/S, and the internal pressure is continuously pressurized to 165MPa;
In the embodiment 2, when the stroke of the press reaches 704mm, the guard ring is bulging to the calibrated size for the first time, the cross beam of the pressure equipment is lifted up quickly and relieved quickly, the instability phenomenon caused by unstable internal pressure due to discontinuous spraying of the hydraulic medium or uneven local leakage of the liquid is avoided, blank size data in the stable bulging stage are monitored in real time through a visual displacement sensor, and the instability phenomenon of the shape such as bulging, concave waist or loudspeaker does not occur;
And after the first-pass bulging is finished, replacing a hydraulic bulging die with the diameter of 1300mm for the force-reducing column to perform second-pass bulging. The die mounting repeats the above step S4. During hydraulic bulging, the initial bulging stage is rapidly loaded, the pressure in the hydraulic medium is rapidly increased from 0 to 150 MPa, and the loading rate of the upper punch is controlled to be 14 mm/s. In the steady bulging stage, the loading speed of the upper punch is as stable as possible at 18 mm/s, and the internal pressure is gradually increased to 178 MPa. When the stroke of the press reaches 500 mm, the guard ring is expanded to the calibrated size in the second pass, and the pressure equipment beam is quickly lifted and quickly relieved. The blank size data is monitored in real time through a visual displacement sensor, so that the instability phenomenon does not occur;
S5-3, unloading, namely expanding the blank to a calibrated size when the pressure equipment reaches a preset stroke, rapidly lifting the pressure equipment beam, rapidly releasing pressure, and completing hydraulic expansion of the blank to obtain the hydraulic expansion thick-wall cylinder. And after unloading, measuring the size of the blank, wherein the bus bar of the blank is straight and reaches a preset size, specifically, the outer diameter is 2060 mm, the inner diameter is 1830 mm, the wall thickness is 115mm, the height is 1016mm, and the hydraulic bulging is finished.
On the basis, a detecting instrument is adopted to detect the diameter, the wall thickness and the roundness of the hydraulic bulging thick-wall cylinder, unqualified parts are adjusted according to the instability phenomenon, then bulging is carried out again until the products are detected to be qualified, the subsequent processing procedure is carried out, and finally the thick-wall cylinder forge piece such as the non-magnetic retaining ring of the 1000MW steam turbine generator meeting the requirements is obtained.
The foregoing is merely illustrative of the present invention, and the present invention is not limited thereto, and any changes or substitutions easily contemplated by those skilled in the art within the scope of the present invention should be included in the scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.