CS206746B1 - Shoe upper and method of its manufacture - Google Patents

Shoe upper and method of its manufacture Download PDF

Info

Publication number
CS206746B1
CS206746B1 CS55779A CS55779A CS206746B1 CS 206746 B1 CS206746 B1 CS 206746B1 CS 55779 A CS55779 A CS 55779A CS 55779 A CS55779 A CS 55779A CS 206746 B1 CS206746 B1 CS 206746B1
Authority
CS
Czechoslovakia
Prior art keywords
weight
plastisol
casting
polyvinyl chloride
layer
Prior art date
Application number
CS55779A
Other languages
Czech (cs)
Inventor
Jiri Varhanik
Milos Spetla
Jaroslav Mikula
Jan Stetkar
Stanislav Fetrik
Slavko Hudecek
Jaroslav Hnidek
Original Assignee
Jiri Varhanik
Milos Spetla
Jaroslav Mikula
Jan Stetkar
Stanislav Fetrik
Slavko Hudecek
Jaroslav Hnidek
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jiri Varhanik, Milos Spetla, Jaroslav Mikula, Jan Stetkar, Stanislav Fetrik, Slavko Hudecek, Jaroslav Hnidek filed Critical Jiri Varhanik
Priority to CS55779A priority Critical patent/CS206746B1/en
Publication of CS206746B1 publication Critical patent/CS206746B1/en

Description

(54) Svršek obuvi a způsob jeho výroby(54) Footwear upper and method of its manufacture

Vynález se týká svršku obuvi, složeného z vnitřní textilní vrstvy a střední a vnější vrstvy na bázi polyvinylchloridu, který se vyznačuje výraznou sorpcí vodních par z vnitřní strany a nepropustností pro vodu z vnější strany a způsobu jeho výroby.The invention relates to a shoe upper composed of an inner textile layer and a middle and an outer layer based on polyvinyl chloride, characterized by a significant water vapor sorption from the inside and an impermeability to the water from the outside and a process for its manufacture.

Odlévaná obuv je používána především jako dámská kozačková a dětská obuv, a nahrazuje obuv koženou. Vzhledem k nepropustnosti pro vodu z vnější strany a vyhovující mechanické vlastnosti ,se jeví výhodnější než kožená obuv. Velkou nevýhodou jsou naprosto nedostačující hygienické vlastnosti. Odlévaná obuv je v současné době vyráběna dvojnásobným naléváním plastisolu polyvinylchloridu do duté předehřáté formy, přičemž pro obě nalévání se používá shodné receptury. Pro odlévání plastisolů, želatinaci a separaci sé k odlitku připevní textilní podšívková vrstva a z vnější strany se provede nástřik povrchové úpravy. Takto vyrobená odlévaná obuv je nepropustná pro vodní páru a postrádá sorpční vlastnosti.Cast shoes are used primarily as women's boots and children's shoes, and replace leather shoes. Due to the impermeability to water from the outside and satisfactory mechanical properties, it appears to be more advantageous than leather shoes. A great disadvantage is the absolutely inadequate hygienic properties. The cast footwear is currently produced by pouring polyvinyl chloride plastisol twice into a hollow preheated mold, using the same recipe for both pouring. To cast the plastisols, the gelatinization and separation are attached to the casting by a textile lining layer and a coating is applied from the outside. The cast footwear thus produced is impervious to water vapor and lacks sorption properties.

Pro zvýšení sorpčních vlastností odlévané obuvi z polyvinylchloridu nelze použít hydrofilní látky jako škrob, viskózu, kasein, želatinu, agar-agar, estery, estery celulózy, které jsou uvedeny v NSR patentovém spisu č. 967 903, britském 1 277 438, USA 3 249 465, švýcarském 353 897 a čs. 145 001. Tyto látky nelze použít, pro zvýšení sorpčních vlastností odlévané obuvi z důvodů bud nízké sorpční kapacity, nebo pro technologii odlévání nevyhovujícího viskozitního chování plastisolu s přídavkem těchto látek. Nevýhodou je rovněž relativně snadné vyluhování hydrofilních látek ve styku s vodou.Hydrophilic substances such as starch, viscose, casein, gelatin, agar-agar, esters, cellulose esters, which are disclosed in German Patent Specification No. 967 903, British 1 277 438, U.S. Pat. 465, Swiss 353 897 and MS. 145 001. These substances cannot be used for increasing the sorption properties of cast shoes due to either low sorption capacity or for casting technology of unsatisfactory viscosity behavior of plastisol with the addition of these substances. A disadvantage is also the relatively easy leaching of hydrophilic substances in contact with water.

Stejně nevýhodné se jeví použití práškového polyvinylalkoholu podle švýcarského patentu č. 328 436 a NSR patentu č. 1 614 960.Equally disadvantageous is the use of polyvinyl alcohol powder according to Swiss Patent No. 328,436 and German Patent No. 1,614,960.

Je známo řešení zvýšení navlhavosti přídavkem kolagenních vláken (ěs. patenty č. 141 625 a 137 947) nebo brusného prachu ze syntetických usní (čs. patent č. 136 332). Oba způsoby, mimo jiné nevýhody, mají jen omezený význam vzhledem k tomu, že se jedná o přídavek odpadních materiálů, jejichž výskyt je závislý na vyráběném ' množství a způsobu zpracování přírodních a syntetických usní.It is known to increase the wettability by adding collagen fibers (U.S. Pat. Nos. 141,625 and 137,947) or abrasive dust of synthetic leather (U.S. Pat. No. 136,332). Both methods, among other disadvantages, are of limited importance since they involve the addition of waste materials, the occurrence of which depends on the quantity produced and the method of processing natural and synthetic leather.

Popis vynálezu k čs. AO č. 157 212 uvádí způsob výroby tenkostěnných útvarů z plastů různými technologiemi, spočívající na principu, že se k zpracovávanému materiálu přidá plnivo nebo směs plniv na bázi makromolekulámích látek nerozpustných ve vodě, obsahujících polární skupiny schopné vázat vodu. Při uvedeném způsobu výroby se dosahuje v závislosti na přidávaném množství plniv zvýšení sorpce vodních par. Použití hydrofilních plniv do vnější vrstvy však způsobuje podstatnéDescription of the invention to MS. AO No. 157 212 discloses a process for producing thin-walled plastics by various technologies, based on the principle that a filler or a mixture of fillers based on water-insoluble macromolecular substances containing polar groups capable of binding water is added to the material to be treated. In the production process, the water vapor sorption is increased depending on the amount of fillers added. However, the use of hydrophilic fillers in the outer layer is essential

• V ti snížení odolnosti v ohybu při současném vzniku bílého lomu, který působí jako vzhledová závada. Mimo to při použití tohoto postupu vykazuje i odlévaná obuv nehomogenní povrch, což je způsoí beno vysokým obsahem sorbóvané vody v plnivu.• Reducing the bending resistance while producing a white fracture that acts as a visual defect. In addition, cast shoes have an inhomogeneous surface, which is due to the high content of sorbated water in the filler.

Uvedené nevýhody odstraňuje svršek obuvi ; složený z vnitřní textilní vrstvy a střední a vnější vrstvy na bázi PVC s obsahem změkčovadla, ' stabilizátorů aj. podle vynálezu, jehož podstatou je, že střední vrstva svršku o tloušťce 1,0 až 2,0 mm í obsahuje 10 až 40 % hmot., vztaženo na hmotnost j polymeru, statisticky rozptýlených síťovaných i makromolekulárních látek, připravených polyme| raci směsi vinylických monomerů a obsahujících i polární skupiny, jako jsou skupiny hydroxyloyé, amidové a karboxylové v H+, Na+ a K+ forměíThese disadvantages are eliminated by the upper of the shoe; % comprising a textile inner layer and a middle and outer PVC-based layer containing a plasticizer, stabilizers, etc. according to the invention, the central layer of the upper having a thickness of 1.0 to 2.0 mm containing 10 to 40 wt. , based on the weight j of the polymer, statistically dispersed cross-linked and macromolecular substances, prepared by polymer | The reaction of a mixture of vinyl monomers and also containing polar groups such as hydroxyloyed, amide and carboxyl groups in H + , Na + and K + forms

Svršek obuvi podle vynálezu se vyrábí odléváúím plastisolu polyvinylchloridu do duté formy, jeho želatinaéí a následnou separací odlitku, ke kterému se připevní textilní vrstva. Podstatou způsobu výroby podle vynálezu je, že se odlévání plastisolu provádí ve dvou operacích, přičemž se nejprve odlévá plastisol polyvinylchloridu s obsahem běži ných přísad a dále 10 až 40 % hmot., vztaženo na ! hmotnost polymeru, statisticky rozptýlených mak, romolekulámích látek, připravených polymerací směsi vinylických monomerů a obsahujících polární skupiny, jako skupiny hydroxylové, amidové a karboxylové, s výhodou karboxylové skupiny ve formě H+, Na+ a K+ a dále 0,1 až 2,0 % hmot., vztaženo na hmotnost síťované makromolekulám! látky, sorbované vody.The shoe upper according to the invention is produced by casting polyvinyl chloride plastisol into a hollow mold, its gelatin and subsequent separation of the cast to which the textile layer is attached. The essence of the process according to the invention is that the casting of plastisol is carried out in two operations, firstly casting plastisol of polyvinyl chloride with the content of customary additives and furthermore 10 to 40 wt. weight of polymer, statistically dispersed poppy, romolecular substances prepared by polymerizing a mixture of vinyl monomers and containing polar groups such as hydroxyl, amide and carboxyl groups, preferably carboxyl groups in the form of H + , Na + and K +, and further 0.1 to 2, 0% by weight, based on the weight of the cross-linked macromolecules! substances, sorbed water.

Odlévaná obuv z textilu a polyvinylchloridu podle vynálezu se ve srovnání s dosud známou a vyráběnou odlévanou obuví vyznačuje zvýšenou schopností pohlcovat vodní páru při současném zachování flexibility materiálu při namáhání na ohyb. Použitím síťovaných makromolekulárních látek pouze ve vnitřní vrstvě polyvinylchloridu byl rovněž odstraněn nežádoucí bílý lom. 'The textile and polyvinylchloride molded footwear according to the invention has an increased ability to absorb water vapor compared to the known and manufactured molded footwear while maintaining the flexibility of the material when subjected to bending stress. By using cross-linked macromolecular substances only in the inner layer of polyvinyl chloride, unwanted white refraction was also removed. '

U odlévané obuvi podle vynálezu je nejvhodněj! ší volit tloušťku vnitřní polyvinylchloridóvé vrstvy v rozmezí 1,0 až 2,0 mm, což je 2 až 2O.krát více než i tloušťka vnější polyvinylchloridové vrstvy. Vnější vrstva o tloušťce 0,10 až 0,50 min naprosto dostatečně zaručuje něpropustnost pro vodu z vnější strany a dobré mechanické vlastnosti. Tloušťka vnitřní vrstvy je dána množstvím požadované sorbující se vody a -obsahem síťované makromolekulám! látky. Vhodnou volbou množství síťované makromolekulám! látky v polyvinylchloridu i a tloušťky vnitřní vrstvy se dosáhne maximálního sorpčního efektu. Z důvodu maximálního využití i sorpční kapacitý síťované makromolekulámí látky, i je nutno, aby tato byla v polyvinylchloridové vrstvě rozložena statisticky.The molded shoe according to the invention is most suitable. the thickness of the inner polyvinyl chloride layer is 1.0 to 2.0 mm, which is 2 to 20 times more than the thickness of the outer polyvinyl chloride layer. The outer layer with a thickness of 0.10 to 0.50 min guarantees sufficient water impermeability and good mechanical properties. The thickness of the inner layer is given by the amount of sorbent water required and the content of cross-linked macromolecules! substances. Appropriate choice of the amount of cross-linked macromolecules! and the thickness of the inner layer achieves maximum sorption effect. Due to the maximum utilization of the sorption capacity of the cross-linked macromolecular substance, it is necessary that it be statistically distributed in the polyvinyl chloride layer.

ί Protože síťované makromolekulámí látky, které jsou svým charakterem vysoce hydrofilní, sorbují Iv závislosti na relativní vlhkostí vzduchu při manipulačních procesech spájených s jejich výrobou, tj. při mletí, sušení, > adjustaci, balení a skladování, vodní páru, je nutno přeď použitím těchto látek snížit obsah sorbované vody pod 2 % hmot., | j vztaženo na hmotnost síťované makromolekulám! I látky. Vyšší obsah sorbované vody způsobuje Inehomogennost vrstvy, vznik puchýřu a místní' separování od vnější vrstvy.ί Since crosslinked macromolecular substances, which by their nature are highly hydrophilic, absorb even water vapor depending on the relative humidity in the handling processes associated with their production, ie grinding, drying,> adjusting, packaging and storage, water vapor, substances to reduce the sorbed water content below 2% by weight, j based on the mass of the cross-linked macromolecules! I of the substance. Higher sorbed water content results in layer inhomogeneity, blister formation and local separation from the outer layer.

Pro lepší objasnění podstaty vynálezu uvádíme i několik příkladů provedení.In order to better elucidate the essence of the invention, several examples are given.

! Příklady byly provedeny podle následujících postupů:! The examples were performed according to the following procedures:

— příprava plastisolů j- preparation of plastisols j

Plastisoly na bázi polyvinylchloridu byly připraj ‘ Iveny na rychlomíchaČce při 1000 ot/min — složení plastisolů — plastisol pro vnější vrstvu (1. nalévám) suspenzní pastotovomý polyvinylchlorid o K = 70. ftalátové změkčovadlo o střední gelovací schopnosti (např. dioktylftalát) Stabilizátor na bázi bamatých a zinečnatých solí pigmenty — plastisol pro vnitřní vrstvu (2. nalévání) ' suspenzní pastotvomý polyvinylchlorid o K = 70 emulzní pastotvorůý polyvinylchlorid o K = 68 Malátové změkčovadlo hmot. dílů hmot. dílů až 2 hmot. díly 1 až 2 hmót. díly >' hmot. dílů hmot. dílů střední gelovací schopnosti í (např. dioktylftalát) 100 až 120 hmot. dílů stabilizátor na bázi bamatých a zinečnatých solí 1 až 2 hmot. díly pigmenty 1 až 2 hmot. díly síťované makromolekulární látky 10 až 40 hmot. dílůThe polyvinyl chloride-based plastisols were prepared on a high-speed mixer at 1000 rpm - plastisol composition - plastisol for the outer layer (1. pour) suspension paste-form polyvinyl chloride of K = 70th phthalate plasticizer of medium gel ability (eg dioctyl phthalate) Membrane and zinc salts Pigments - Plastisol for inner layer (2nd pouring) Suspension pasty polyvinyl chloride o K = 70 Emulsion paste polyvinyl chloride o K = 68 Malate plasticizer mass. parts by weight parts up to 2 wt. parts 1 to 2 wt. parts> wt. parts by weight parts (eg dioctyl phthalate) of 100 to 120 wt. parts stabilizer based on barium and zinc salts 1 to 2 wt. parts pigments 1 to 2 wt. parts of crosslinked macromolecular substance 10 to 40 wt. parts

Síťované makromolekulámí látky jsou dávkovány do plastisolu ve formě předsměsi ve změkčo. vadle.The cross-linked macromolecular substances are dosed into plastisol in the form of a masterbatch into a softener. vadle.

— postupy při přípravě odlévané obuvi 1/ Dutá forma, předehřátá na teplotu 120 ažProcesses for the preparation of cast shoes 1 / Hollow mold preheated to a temperature of 120 to

140 °C, se naplní plástisolem pro vnější vrstvu a pó jeho vylití se vzniklá vrstva o tloušťce 0,1 a£ 0,5 mm předželatinuje při teplotě 200 °G. Potom se do formy naleje platisol pro vnitřní vrstvu a po jeho vylití se vzniklý dvouvrstvý útvar podrobí želatinaci při teplotě 200 až 250 °C a po jeho vyjmutí z formy se k němu připevní podšívka.140 [deg.] C., is filled with sheathing for the outer layer and the poured layer is pre-gelatinised at a temperature of 200 [deg.] C. and 0.1 to 0.5 mm thick. Platisol for the inner layer is then poured into the mold and, after pouring, the resulting two-layer formation is gelatinized at a temperature of 200 to 250 ° C and, after its removal from the mold, the lining is attached thereto.

. 27 Dutá forma, předehřátá na teplotu 120 až 140 °C, se naplní plástisolem pro vnější vrstvu a po jeho vylití se opět forma naplní plástisolem pro vnitřní vrstvu. Forma s plástisolem se zahřeje na' 200 °C a po vylití se vzniklý dvouvrstvý útvar. The hollow mold, preheated to a temperature of 120 to 140 ° C, is filled with the sheath for the outer layer and after pouring, the mold is again filled with the sheath for the inner layer. The honeycomb mold is heated to '200 ° C and the two-layer formation formed after pouring

i. podrobí želatinaci při teplotě 200 až 250 °G a po I jeho vyjmutí z formy se k němu připevní podšívka, j - parametry uváděné v příkladech k charakterizování odlévané Obuvi:i. subjected to gelatinization at a temperature of 200 to 250 ° C, and after its removal from the mold, the lining is attached thereto; j - the parameters given in the examples to characterize the molded footwear:

! — tloušťka, .— plošná hmotnost, — navlhavost, ΐ_ — vysýchavost,! - thickness, .— basis weight, - moisture, ΐ_ - drying,

I - odolnost proti opakovanému ohybu. >I - repeated bending resistance. >

) Navlhavost, vysýchavost ' í) Moisture, drying out

Navlhavost je definována jako schopnost mate- ! riálu přijímat vodní páru. Měrnou jednotkou je ;(mg.cm2). Vysýchavost je schopnost materiálu uvolňovat přijatou vodní páru.Moisture is defined as the ability to mate! water vapor. The unit of measure is ; (mg.cm 2 ). Drying is the ability of a material to release water vapor.

' Měrnou jednotkou je procento hmotnostní.The unit of measure is the percentage by weight.

Odolnost proti opakovanému ohybuResistance to repeated bending

Odolnost proti opakovanému ohybu je defino-; vána jako schopnost materiálu klást odpor proti ' i mechanickému poškození při opakovaném ohýbái ní. Vyhodnocuje se při zvoleném počtu ohybů ! v kilocyklech a vyjadřuje ve stupních odolnosti 1 až i 5. ’ > 5 — zkušební těleso je bez porušeníResistance to repeated bending is defino-; It is referred to as the ability of the material to resist mechanical damage during repeated bending. It is evaluated at the selected number of bends! in kilocycles and expresses in resistance grades 1 to 5. '5 - the test specimen is intact

- 4 — trhliny v povrchové úpravě i 3 — vznik trhlin v délce do 1 mm — vznik trhlin v délce od 1 mm_____________ 1 — trhliny až k podkladu nebo celou tloušťkou ] zkušebního tělesa. . ! l·' · ' !- 4 - cracks in surface finish i 3 - cracks up to 1 mm long - cracks up to 1 mm long _____________ 1 - cracks to the substrate or full thickness] of the specimen. . ! l · '·'!

Příklady i až 3 í Podle prvního postupu a na bázi receptur pro vnější a vnitřní vrstvu byly připraveny pouze vzorky odlitků bez textilní podšívky. Síťovaná makromolekulám! látka ve vnější vrstvě se lišila obsahem sorbované vody, který je udán v hmot- , nostních procentech, vztažených na hmotnost síťo- j váné makromolekulám! látky. j __Vyhodnocení je uvedeno v tabulce I. j : . :.i ’ 'EXAMPLES 1 to 3 According to the first process and based on recipes for the outer and inner layers, only cast samples without textile lining were prepared. Meshed macromolecules! the substance in the outer layer differed in the content of sorbed water, which is given in weight percent, based on the mass cross-linked by macromolecules! substances. The evaluation is shown in Table. : .i ’'

Tabulka č. I — k příkladům 1 až 3Table I - Examples 1 to 3

Příklad * Vzhled povrchu nánosů PVCExample * Surface appearance of PVC deposits

1 1 0,4 0.4 Hladký, bez puchýřů Smooth, blister-free 2 2 2,2 2.2 Vnitřní vrstva — místy drobné puchýře a místní odseparování od vnější vrstvy Inner layer - in places small blisters and local separation from the outer layer 3 3 4,3 4.3 Vnitřní vrstva — drobné puchýře v celé ploše a odseparování od vnější vrstvy ve větším rozsahu než v případě 2 Inner layer - small blisters over the entire surface and separation from the outer layer to a greater extent than in case 2

Z příkladů 1 až 3 plyne, že k výrobě odlévané obuvi podle vynálezu je nutno použít síťovanou i makromolekulami látku s obsahem sorbované [ vody do 2 % hmot. ' i . ..._______________ ... . ____ IExamples 1 to 3 show that a crosslinked and macromolecular substance having a sorbed [water content of up to 2% by weight] must be used to produce the molded shoe according to the invention. 'i. ..._______________ .... ____ I

Příklady 4 až 11 { Examples 4-11 {

J V příkladech 4 až 11 byly připraveny vzorky | í odlévané obuvi, podle postupu ě. 1, které se lišily | ; obsahem síťované makromolekulami látky póly| métakrylanu sodného síťovaného 20 % Έΐνίη^-Π benzenu s obsahem 0,3 % hmot. sorbované vody i v jednotlivých vrstvách. Obsah síťované makromolekulámí látky je udán v % hmot., vztažených na hmotnost polymeru. Jako podšívkový materiál byl · použit polyamidový úplet s nalaminovanou póly- i uretanovou pěnou. iIn Examples 4 to 11, samples were prepared shoes, according to the procedure. 1, which differed ; content of cross - linked macromolecules % sodium methacrylate crosslinked with 20% by weight of benzene containing 0.3 wt. sorbed water even in individual layers. The content of the cross-linked macromolecular substance is given in% by weight, based on the weight of the polymer. A polyamide knit with laminated poles and urethane foam was used as lining material. and

Naměřené hodnoty jsou uvedenyv tabulce č. II.The measured values are given in Table II.

Tabulka č. II — k příkladům 4 až 11 i .Table II - Examples 4 to 11 i.

Obsah síťované makromol. látky v plastisolu pro vnitřní vrstvu vnější vrstvu (% hmot.) (% hmot.) The content of the networked macromol. substances in plastisol for inner layer outer layer (% by weight) (% by weight) Parametry vnitřní vrstvy Parameters of inner layer Parametry vnější vrstvy Parameters of the outer layer Příkl. Ex. tloušťka (mm) thickness (mm) plošná hm. (kg.m-2)flat mass (kg.m- 2 ) tloušťka (mm) thickness (mm) plošná hm. (kg.m-2)flat mass (kg.m- 2 ) 4 4 0 0 0 0 1,52 1.52 1,92 1.92 0,15 0.15 0,181 0.181 5 5 10 10 0 0 1,68 1.68 2,03 2.03 0,35 0.35 0,401 0.401 6 6 20 20 May 0 0 1,75 1.75 2,15 2.15 0,21 0.21 0,263 0.263 7 7 30 30 0 0 1,46 1.46 1,83 1.83 0,18 0.18 0,210 0.210 8 8 40 40 0 0 1,59 1.59 1,87 1.87 0,37 0.37 0,397 0.397 9 9 20 20 May 10 10 1,67 1.67 1,95 1.95 0,39 0.39 0,429 0.429 10 10 20 20 May 20 20 May 1,71 1.71 2,08 2.08 0,23 0.23 0,270 0.270 11 11 20 20 May 30 30 1,65 1.65 1,98 1.98 0,29 0.29 0,315 0.315

Pokračování tabulky č. II — k příkladům 4 až 11 Parametry vzorků odlévané obuviContinuation of Table II - Examples 4 to 11 Parameters of cast shoe samples

Příkl. Ex. Navlhavost (mg. cm-2)Moisture (mg. Cm -2 ) Vysýchavost (%) Drying (%) Odolnost proti opak. ohybu po 150 kc Opposite Resistance bending after 150 kc Vzhled po opakovaném ohýbání Appearance after repeated bending 4 4 3,1 3.1 95 95 5 . 5. beze změny unchanged 5 5 6,9 6.9 81 81 5 5 beze změny unchanged 6 6 12,1 12.1 87 87 5 5 beze změny unchanged 7 7 16,5 16.5 79 79 5 5 beze změny unchanged 8 8 19,8 19.8 80 80 4 4 beze změny unchanged 9 9 13,3 13.3 76 76 3 3 nepatrná barevná změna v místě ohybu slight color change at the bend 10 10 15,1 15.1 73 73 2 2 výrazná barevná změna v místě ohybu Significant color change at the bend 11 11 18,7 18.7 79 79 1 1 výrazná barevná změna v místě ohybu Significant color change at the bend

Z příkladů 4 až 11 je zřejmý pozitivní vliv síťované makromolekulám! látky na hygienické ; vlastnosti odlévané obuvi. Její obsah ve vnější vrstvě zvyšuje hodnotu navlhavosti, avšak negativně se projevuje na odolnosti materiálu proti ohybu.Examples 4 to 11 show the positive effect of cross-linked macromolecules! hygienic substances; characteristics of cast shoes. Its content in the outer layer increases the wetting value but has a negative effect on the bending resistance of the material.

Její obsah ve vnitřní vrstvě je limitován viskozitními požadavky na plastisol pro vnitřní vrstvu vyplývajícími z technologie odléváni, i Příklady 12 až 15 i Podle postupu č. 2 byly připraveny vzorky podlévané obuvi, které se lišily typem síťované ,! makromolekulám! látky ve vnitřní vrstvě. Všechny aplikované látky byly síťovány 20 % divinylbenzenu. Plastisol pro vnitřní vrstvu obsahoval 20 % Ihmot. síťované makromolekulám! látky, vztažei ných na hmotnost polymeru, plastisol pro vnější j vrstvu byl bez síťované makromolekulámí látky.Its content in the inner layer is limited by the viscosity requirements for plastisol for the inner layer resulting from the casting technology. Examples 12 to 15 i According to procedure 2, samples of lined footwear were prepared which differed in the type of mesh . macromolecules! substances in the inner layer. All applied substances were crosslinked with 20% divinylbenzene. Plastisol for the inner layer contained 20% by weight. networked macromolecules! The plastisol for the outer layer was free of cross-linked macromolecular substances.

; Jako podšívkový materiál byl použit polyamidový· i úplet s nalaminovanou polyuretanovou pěnou.; A polyamide knit with a laminated polyurethane foam was used as lining material.

Výsledky jsou uvedeny v tabulce ě. III.The results are shown in Table. III.

Z příkladů 12 až 15 vyplývá, že pro odlévanou obuv podle vynálezu je nejvhodnější jako síťovaná makromolekulámí látka polyakrylan Sodný apolymetakrylan sodný. Uvedené příklady rovněž potvrzují účinek síťované makromolekulámí látky pro odlévanou obuv vyrobenou tzv. „stúdeným odléváním“.Examples 12 to 15 show that sodium polyacrylate and sodium polyacrylate are best suited as the crosslinked macromolecular substance for the shoe according to the invention. The examples also confirm the effect of the cross-linked macromolecular substance on the molded footwear produced by the so-called "cold casting" process.

Claims (2)

PŘEDMĚTSUBJECT VYNÁLEZU ' 1. Svršek obuvi složený z vnitřní textilní vrstvy ! střední a vnější vrstvy na bázi polyvinylchloridu s obsahem změkčovadla, stabilizátorů, barviv a popřípadě dalších běžných přísad, vyznačený tím, že jeho střední vrstva o tloušťce 1,0 až 2,0 mm obsahuje 10 až 40 % hmotnostních, vztaženo na hmotnost polymeru, statisticky rozptýlených síťovaných makromolekulámích látek, připravených polymerací směsi vinylických monomerů a obsahu- jících polární skupinyjako jsou skupiny hydroxylové, amidové a karboxylové v H+, Na+ a K+ formě.SUMMARY OF THE INVENTION 1. A shoe upper composed of an inner textile layer! middle and outer layers based on polyvinyl chloride containing a plasticizer, stabilizers, colorants and optionally other conventional additives, characterized in that its middle layer of 1.0 to 2.0 mm thickness contains 10 to 40% by weight, based on the weight of the polymer, statistically scattered cross-linked macromolecular substances prepared by polymerizing a mixture of vinyl monomers and containing polar groups such as hydroxyl, amide and carboxyl groups in H + , Na + and K + form. 2. Způsob výroby svršku obuvi podle bodu 1 odléváním plastisolu polyvinýlchloridu s obsahem změkčovadla, stabilizátorů, barviv a popřípadě dalších přísad do duté formy, želatinací, vyjmutím odtlitku a připevněním textilní vrstvy, vyznačený tím, že odlévání plastisolu se provádí ve dvou operacích, přičemž nejprve se odlévá plastisol polyvinylchloridu s obsahem běžných přísad a, dále 10 až 40 % motnostních, vztaženo na hmotnost polymeru, statisticky rozptýlených makromolekulámích látek, připravených polymerací směsi vinylických monomerů a obsahujících polární skupiny; jako skupiny hydroxylové, amidové a karboxylové; s výhodou karboxýlové skupiny ve formě H+, Na+ a K+, a dále 0,1 až 2,0 % hmotnostního, vztaženq na hmotnost síťované makromolekulámí látky; sorbované vody.2. A method for producing the shoe upper according to claim 1 by casting plastisol of polyvinyl chloride containing plasticizer, stabilizers, dyes and optionally other additives into a hollow mold, by gelatinizing, removing the casting and attaching a textile layer, characterized in that casting plastisol is carried out in two operations. casting polyvinyl chloride plastisol containing conventional additives and, further, 10 to 40% by weight of polymer, statistically dispersed macromolecular substances prepared by polymerizing a mixture of vinyl monomers and containing polar groups; as hydroxyl, amide and carboxyl groups; preferably carboxyl groups in the form of H + , Na + and K + , and further 0.1 to 2.0% by weight, based on the weight of the cross-linked macromolecular substance; sorbované vody.
CS55779A 1979-01-25 1979-01-25 Shoe upper and method of its manufacture CS206746B1 (en)