CS233468B1 - Concretes and melts for work at negative temperatures - Google Patents

Concretes and melts for work at negative temperatures Download PDF

Info

Publication number
CS233468B1
CS233468B1 CS551782A CS551782A CS233468B1 CS 233468 B1 CS233468 B1 CS 233468B1 CS 551782 A CS551782 A CS 551782A CS 551782 A CS551782 A CS 551782A CS 233468 B1 CS233468 B1 CS 233468B1
Authority
CS
Czechoslovakia
Prior art keywords
mixture
urea
strength
freezing
efflorescence
Prior art date
Application number
CS551782A
Other languages
Czech (cs)
Slovak (sk)
Inventor
Zdenek Bruthans
Juraj Gustafik
Original Assignee
Zdenek Bruthans
Juraj Gustafik
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Zdenek Bruthans, Juraj Gustafik filed Critical Zdenek Bruthans
Priority to CS551782A priority Critical patent/CS233468B1/en
Publication of CS233468B1 publication Critical patent/CS233468B1/en

Abstract

Vynález rieái problém betonáže za záporných teplOt. Pre seaeůsenie zarzautia betonových zmesi a mált ea užíval doposial’ ohřev, 8o je náročné energeticky aj převédzkovo alebo přísady najma chloridov a karbonétov připadne iných solí, Využitie týchto přísad pri vysokých dávkách, ktoré aú pre zamedzenis zmrznuti» vody nutné, limituje ich negativny vplyv na koroziu výstuže, nežiadúce urýchlovanle tuhnutia, ktoré sťažuje spracovanie zmesi, zníženie konečných pevností a tvorba výkvetov. Zasaedzenie zmrznutie ja možné tiež prídavkom močoviny. Vyžaduje vžak tiež vysokú dávku přísady, vedie k vzniku výkvetov a narestenie počistočnej pevnosti je pomalé. Podobné je tomu pri přídavku močoviny a dusičnanu vápenatého. Podle vynálezu se zamedzuje zmrznutie zmesi bez urýchlenia tuhnutia a dosahuje rýchly rast pevnosti za trvalo záporných tepldt bez negativného vplyvu na konečnú pevnost a bez vzniku výkvetov tým, že betonová směs obsahuje relativné nízký súfiasný prídavok iao8oviny β najisenej jednej vodorozpustnej s výhodou alkalickej soli bežne dostupných kyselin ako kyseliny sírovéj, solkiej, uhliSitej, mrave®j, Stavelovej alebo alkalickéj soli, kyseliny dusičnej alebo zmes týchto solí, pričois hmotnostný poměr aeSoviny e rozpnstnej soli. je 1:10 ež 5'0,1,The invention solves the problem of concreting at negative temperatures. For the hardening of concrete mixtures and mortars, heating has been used so far, which is both energy-intensive and operationally demanding, or additives, especially chlorides and carbonates or other salts. The use of these additives at high doses, which are necessary to prevent water freezing, limits their negative impact on reinforcement corrosion, undesirable accelerated solidification, which makes the mixture difficult to process, a decrease in final strength and the formation of efflorescence. Freezing is also possible by adding urea. However, it also requires a high dose of the additive, leads to the formation of efflorescence and the increase in the final strength is slow. The same is true for the addition of urea and calcium nitrate. According to the invention, freezing of the mixture is prevented without accelerating solidification and a rapid increase in strength is achieved at permanently negative temperatures without a negative effect on the final strength and without the formation of efflorescence, by the concrete mixture containing a relatively low simultaneous addition of a β-compound dissolved in one water-soluble, preferably alkaline salt of commonly available acids such as sulfuric, hydrochloric, carbonic, formic, staval or alkaline salt, nitric acid or a mixture of these salts, whereby the weight ratio of the compound to the soluble salt is 1:10 to 5:0.1,

Description

233466 2233466 2

Vynález se týká betónov a mált pře práce za nízkých tepldt najma v stavebníctve.The invention relates to concretes and low-temperature work especially in construction.

Betony a malty užívaná za zápornýh tepldt nesmá zmrznut v čerstvom stave, aby. bolomožné leh normálně dopravovanle, ukládánie a spracovanie. Nesmú vykazovat rýchle tuhnutie,ktoré by stažovalo rozvoz a spracovanie. Po uložení musí zmes tvrdnut aj za zápornýchtepldt. Nle je vyhovujúce, aby pevnost rástla až po přechode záporných tepldt. To spo-maluje postup stavebných práč a dochádza tiež k vysyehaniu zmesi před vytvrdnutím. Vy-schnutá zmes nezatvrdne pri nedostatku vody ani po příchodu kladných tepldt. Zmrznutiebetonu v době tuhnutia a počiatočného tvrdnutia - kedy pevnost je nízká - má za následoktrvalá porušenie - zníženie pevnosti, ktorá nedosiahne projektovaná hodnotu ani podlhom čase v prostředí kladných tepldt. , Příčinou je poruéenie Struktúry tvrdnúceho materiálu expanziou, ktorá sprevédza vznikl'adu zo zámesovej vody, Týmto negativným vplyvom nízkých tepldt sa v doterajSej praxibráni jednak ohrevom zložiek zmesi, ohrevom vyrobenéj zmesi a ohrevom konštrukcie, čo jeenergeticky a prevádzkovo náročné, jednak prídavkom látok, ktoré by zabránili zmrznutiezámesovej vody v maltovéj či betónovej zmesi.Concretes and mortars used for negative heat must not be frozen in the fresh state in order to:. it can be easily transported, stored and processed. They must not show rapid solidification, which would reduce delivery and processing. After storage, the mixture must also be hardened to a negative temperature. Nle is good for the strength to grow after the negative heat transition. This reduces the progress of the washing machine and also causes the mixture to dry out before curing. The dry mixture does not harden when water is too low, even after positive temperatures. Freezing of the concrete at the time of setting and initial hardening - when strength is low - has a persistent failure - a reduction in strength that does not reach the projected value even over a long time in a positive heat environment. This is due to the failure of the structure of the hardening material by expansion, which spreved out of the resultant water, by the negative effects of low temperatures in the practice practice of heating the mixture components, heating the mixture and heating the construction, which is both energy and operational, and the addition of substances that would prevent freezing of the water in the mortar or concrete mixture.

Doteraz sá známe najma přídavky na báze chloridov a karbonátov. Tle májá však obmedzenépoužitie. Pro zamedzenie zmrznutia betónovej zmesi pri teplote -10 °G by bolo nutné použitprídavok 6 až 8% týchto látok z hmotnosti cementu. Chloridy však nie je možné použitv takých dávkách vzhTadom na škodlivý vplyv na koróziu výstuže betonu. V dávkách pod 2 5Éz hmotnosti cementu, ktoré sa za určitých podmienok považujú niekedy za přístupné z hla-dí ska korázie, zsbrsňájá zmrznutiu vody v betone iba do -3 °C. Karbonáty v týchto dávkách,ktoré aebránia zmrznutiu zámesovej vody, netolko urýchlujú tuhnutie, že nie je možnéapracovať zmes před tuhnutím.So far, we have known chlorine and carbonate-based additives. However, it has limited use. To prevent freezing of the concrete mixture at -10 ° C, the addition of 6 to 8% of these substances by weight of the cement would be necessary. However, chlorides cannot be used in such doses due to the harmful effect on the corrosion of the concrete reinforcement. In batches below 2 É hmotnosti from the weight of the cement, which is sometimes considered accessible under corrosion under certain conditions, it only increases the freezing of water in concrete up to -3 ° C. Carbonates in these doses, which prevent freezing of the wash water, do not accelerate the solidification that it is not possible to work the mixture before solidification.

Vplyv týchto dávek na konečná pevnost je velmi nepriaznivý, pevnost klesá na zlomokpdvodnej hodnoty. Dochádza aj k intenzívnej tvorbě výkvetov a vzniku nebezpečia alkalickejkorózle. Obdobné negativné vplyvy májá aj přísady iných solí. Podlá čsl. patentu 167 115sa zabraňuje zmrznutiu vody v betónovej zmesi prídavkom karboxyldiamidu triviálně močo-viny. Močovina nezrýchluje tuhnutie a nemá korozívne vplyvy ani neznižuje konečné pev-nosti. Potřebné sá však poměrně vysoké přídavky - na příklad 10 % z hmotnosti cementupři teplote -10 °C. Při týchto prídavkoch dochádza na povrchoch vystavených schnutiuk tvorbě výkvetov. Narastanie pevnosti za záporných tepldt je v prvých dňoch malé.The effect of these doses on the ultimate strength is very unfavorable, the strength decreases to a fractional value. There is also intense bloom formation and danger of alkaline corrosion. Similar negative effects are also caused by other salt additives. Podlá čsl. No. 167,115, it prevents the freezing of water in a concrete mixture by the addition of a carboxyldiamide of trivial urea. Urea does not accelerate solidification and does not have corrosive effects or reduce final strength. However, relatively high additions are required - for example, 10% by weight of the cementupper at -10 ° C. These additions result in efflorescence on surfaces exposed to dryness. The increase in strength at negative temperatures is small in the early days.

Obdobné je nízká pevnost pri přídavku močoviny a vápenatej soli kyseliny dusičnej a jejkombinácií s inými solami " ako je zřejmé aj z příkladu provedenia uvedeného áalej.Similar is the low strength of the addition of urea and the calcium salt of nitric acid and its combination with other salts, as is evident from the example of carrying out this further.

Uvedené nedostatky nemajá cementové betony a malty podl’a vynálezu, ktoré obsahujáv množštve 1 až 20 % z hmotnosti cementu močoviny e najmenej jednu vo vodě rozpustnás výhodou alkalická sol· kyseliny sírovej, solnej, uhličitej, dusitej, mravčej, šťave-lovej alebo alkalická sol’ kyseliny dusičnej alebo zmes týchto soli pričom hmotnostnýpoměr močoviny a rozpustnéj soli je 1:10 až 5:0,1. Příklady provedeniaThe above mentioned drawbacks do not have the cement concrete and mortar according to the invention, which contains from 1 to 20% by weight of urea cement and at least one water-soluble, preferably alkaline salt of sulfuric acid, salt, carbonate, nitrite, formic, oxalic or alkaline salt. nitric acid or a mixture of these salts wherein the weight ratio of urea to soluble salt is 1:10 to 5: 0.1. Examples of implementation

Vyrobila sa cementová malta z' portlandského cementu a normového plesku v hmotnostnompoměre 1:2 a s v/c = 0,5. Obdobné malta sa vyrobila s prídavkom močoviny a s prídavkompřísad podlá vynálezu. Pre zachovaníe ptfvodnej konzistencie sa v týchto prípadoch - vzhle-dem na stekucovacie pdsobenie močoviny - znížil prídavok zámesovej vody a rovnaké množ-stvo aké obnáša prídavok močoviny. Ihneá po vyrobení bolí maltové vzorky uložené dopriestoru s teplotou -10 °C. Po 14 dňoch pri tejto teplote sa stanovila pevnost u častivzoriek. Zvyšné sa premiestnlli do prostredia s teplotou vzduchu +20 °C, kde sa ponechalitvrdnut 14 dní a potom tiež odskášali. Výsledky sá uvedené v tabulke č. 1. Přídavky přísadsa rozumejá % hmotnosti cementu v maltě. 233468A Portland cement cement and standardized slag was produced at a weight ratio of 1: 2 and with v / c = 0.5. A similar mortar was made with the addition of urea and an additive according to the invention. In order to maintain the initial consistency, in these cases, due to the urea-fluidizing effect, the addition of blending water and the same amount of urea addition were reduced. Once produced, mortar samples hurt a space of -10 ° C. After 14 days at this temperature, the particle strength was determined. The remainder were transferred to an air temperature of +20 ° C, where it was left to harden for 14 days and then also removed. The results are given in Table 1. Additive additive means% by weight of cement in the mortar. 233468

Zmes bez přísad zmrzla a stala sa nespracovateTnou. Zmrznutím doSlo k trvalému poško-deniu, ktoré je příčinou, že ani za kladných tepldt nenastal velký prírastok pevnosti akonečná pevnost je nízká. Obdobné zmrzli zmesi s prídavkom 2 % rozpustných solí aj zmess prídavkom 5 % močoviny, ak boli tieto látky přidávané osobitne, teda nie vo vzájemnej kombinácii.The mixture without ingredients was frozen and became unprocessable. Freezing has resulted in permanent damage, which causes even a large increase in strength even under positive temperatures, and the final strength is low. Similarly, the mixtures were mixed with the addition of 2% soluble salts and mixed with the addition of 5% urea when added separately, i.e. not in combination with each other.

Tabulka č. 1Table 1

Zmes v/c Pevnost v tlaku MPa po dobe/teplotaMixture v / c Compressive strength MPa after time / temperature

14 dní/-10 °C +14 drd/+20 °C t^ez přísad 0,5 0,75 10,9 + 10 % močoviny 0,4 3,5 30,7 + 5 % močoviny + 2% NagSO^ 0,45 8,6 27,2 + 5 % močoviny + 2% KgCO-j 0,45 7,5 22,5 + j % močoviny + 2% NaNO^ 0,45 8,3 29,0 + 5 % močoviny + 2% NaNCi^ 0,45 4,4 22,3 + > % močoviny + 2% štavelan sodný 0,45 10,2 26,2 + j % močoviny + 2% mravčan sodný 0,45 8,4 28,7 + 5 % močoviny + 2% dusičnan vápenatý 0,45 2,8 23,514 days / -10 ° C +14 drd / + 20 ° C admixture 0.5 0.75 10.9 + 10% urea 0.4 3.5 30.7 + 5% urea + 2% NagSO ^ 0.45 8.6 27.2 + 5% urea + 2% KgCO-j 0.45 7.5 22.5 + j% urea + 2% NaNO ^ 0.45 8.3 29.0 + 5% urea + 2% NaNCi ^ 0.45 4.4 22.3 +>% urea + 2% sodium oxalate 0.45 10.2 26.2 + j% urea + 2% sodium formate 0.45 8.4 28.7 + 5% urea + 2% calcium nitrate 0.45 2.8 23.5

Zmesi podTa vynálezu teda so súčasným prídavkom 5 % močoviny a 2 % rozpustných solíz hmotnosti cementu nezamrzali ani keá ich teplota klesla na -10 °C, zachovali si pritejto teplote pčvodnú konzistenciu po dobu viac ako 1 hodiny. leh pevnost za trvalozépomej teploty -10 °C je niekoTkonásobkom pevnosti dosiahnutej s prídavkom 10 % močo-viny, ktorý je nezbytný pře zamedzenie zmrznutia, ak sa použije pri tejto teplote mo-čovina samotná. Nedochádza k tvorbě výkvetov. Nenastalo trvalé poškodenie pevnostizmrznutím - po přechodu do kladných teplčt zmesi áalej normálně tvrdnú a dosahujú dvojaž trojnásobok pevnosti zmesi porovnávacej.Thus, with the simultaneous addition of 5% urea and 2% soluble salt of the cement, the compositions of the invention did not freeze and their temperature dropped to -10 ° C, maintaining their original consistency for more than 1 hour. The strength at ambient temperature of -10 ° C is several times the strength obtained with the addition of 10% urea, which is necessary to prevent freezing when urea is used alone at this temperature. There is no efflorescence. There is no permanent damage by freezing - after the transition to positive heats the mixture continues to harden normally and reach twice the strength of the blend.

Pri ponechaní zmesi podlá vynálezu uvedených v příklade tvrdnúť při voTnom uloženína vzduchu v období s kolísáním denných teplčt od -10 °C po 0 °C dosiahli sa v priebehu1 týždňa pevnosti v tlaku až 20,0 MPa a po áalšom vytvrdnutí při normálněj teplote ažvýše 40 MPa. Zmes bez přísad však nedosiahla za rovnakých podmienok pevnost ani 15 MPaa táto pevnost áalej nevzrastá.Allowing the mixture according to the invention cited in the example to cure in a free air deposition during a period of daily temperature fluctuations of -10 ° C to 0 ° C, a compressive strength of up to 20.0 MPa is achieved within 1 week and up to 40 after further curing. MPa. However, the additive-free mixture did not reach a strength of even 15 MPaa under the same conditions and this strength does not increase further.

Pri praktickom využití sa přísady přidávají! do zmesi alebo osobitne alebo vopredspolu zmiešané alebo aj predmiešané s ostatnými zložkami zmesi alebo jej častou - například s cementom. Přísady možno přidat aj vo formě roztoku, spolu so zámesovou vodou aleboosobitne do miešačky. NakoTko prídavkom přísad nastáva silné stekutenie zmesi, třeba prezachovanie predpísanej konzistencie znížiť obsah zámesovej vody a to zhruba hmotnostněekvivalentně přídavku přísad. Iné osobitné opatrenia pri výrobě betónovej zmesi nie súpotřebné. Keáže betonová či maltová zmes nezamrzá, nie je potřebný ohřev zámesovej vodya kameniva pri výrobě zmesi.In practical use, the ingredients are added! into the mixture, or separately or pre-mixed, or even premixed with the other ingredients of the mixture or part thereof - for example, with cement. Additives can also be added in the form of a solution, together with the mixing water or separately in the mixer. Since the addition of additives results in a strong fluidisation of the mixture, it is necessary to overwhelm the prescribed consistency to reduce the content of the mixing water, roughly equivalent to the addition of additives. Other special precautions for the production of concrete mixtures are not necessary. It does not freeze the concrete or mortar mixture, it is not necessary to heat the mixing water and aggregates in the production of the mixture.

VzhPadom na rozdielne podmienky při rdznych využitiach (teplota, obsah vody v zmesi,poměry miešania, aktivnost cementu) aj rozdielne požadavky) nárast pevnosti, spracova-telnost) je účelná určit optimálny prídavok pre konkrétné využitie skusmo, pričom platí,že přídavky nižšie, ako sa vymedzujú na straně 2 neposkytujú už technicky významná účin-nost a přídavky vyššie ako vymedžené na straně 2 mSžu byt sprevádzané nežiaducimi vedlej-šími účinkami.Due to the different conditions of different uses (temperature, water content of the mixture, mixing ratios, cement activity) and different requirements) strength increase, workability), it is expedient to determine the optimal addition for a particular application, while the allowances below as defined on page 2, no longer provide a technically significant efficacy and additions higher than those defined on page 2 may be accompanied by undesirable side effects.

Claims (1)

PREDMET VYNÁLEZUOBJECT OF THE INVENTION Betony a malty pre práce za záporných teplfit vyznačené tým, že obsahujú v množstveConcrete and mortar for work at negative temperatures indicated by the fact that they contain in quantities 1 až 20 % z hmotnosti cementu močoviny a najmenej jednu vodorozpustnú s výhodou alkalickú so! kyseliny sírovej, solnej, uhličitéj, mravčej, Šťavelovej alebo alkalickú sol' kyseliny dusičnéj alebo zmes týchto solí, pričom hmotnostný poměr močoviny a rozpustnej soli j®1 to 20% by weight of urea cement and at least one water-soluble, preferably alkaline, salt; sulfuric, hydrochloric, formic, oxalic or alkaline salts of nitric acid or a mixture of these salts, the weight ratio of urea to soluble salt being 1:10 až 5:0,1.1:10 to 5: 0.1.
CS551782A 1982-07-19 1982-07-19 Concretes and melts for work at negative temperatures CS233468B1 (en)