CS244033B1 - Process for the production of multi-component catalysts for the oxidation of aldehydes - Google Patents

Process for the production of multi-component catalysts for the oxidation of aldehydes Download PDF

Info

Publication number
CS244033B1
CS244033B1 CS847075A CS707584A CS244033B1 CS 244033 B1 CS244033 B1 CS 244033B1 CS 847075 A CS847075 A CS 847075A CS 707584 A CS707584 A CS 707584A CS 244033 B1 CS244033 B1 CS 244033B1
Authority
CS
Czechoslovakia
Prior art keywords
molybdenum
oxidation
paste
optionally
atomic ratio
Prior art date
Application number
CS847075A
Other languages
Czech (cs)
Other versions
CS707584A1 (en
Inventor
Alexandr Martinec
Josef Moravek
Werner Havlicek
Jiri Slavik
Josef Tichy
Jaroslav Machek
Jakub Rosenthal
Petr Opatril
Jaroslava Lukacova
Original Assignee
Alexandr Martinec
Josef Moravek
Werner Havlicek
Jiri Slavik
Josef Tichy
Jaroslav Machek
Jakub Rosenthal
Petr Opatril
Jaroslava Lukacova
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Alexandr Martinec, Josef Moravek, Werner Havlicek, Jiri Slavik, Josef Tichy, Jaroslav Machek, Jakub Rosenthal, Petr Opatril, Jaroslava Lukacova filed Critical Alexandr Martinec
Priority to CS847075A priority Critical patent/CS244033B1/en
Publication of CS707584A1 publication Critical patent/CS707584A1/en
Publication of CS244033B1 publication Critical patent/CS244033B1/en

Abstract

Způsob výroby vícesložkových katalyzátorů pro oxidaci aldehydů na karboxylové kyseliny smísením homogenního vodného roztoku výchozích sloučenin aktivních složek, kterými jsou oxidy molybdenu, vanadu a dalších promotujících kovů z I., V. a VIII. skupiny Mendělejevova periodického systému, ořičemž atomární poměr' molybdenu ku vanadu 2 : 1 až 12 : 1 a atomární poměr promotorů ku molybdenu je 0,01 až 0,5 s organickými hydroxykyselinami zvolenými ze skupiny zahrnující kyselinu vinnou a citrónovou v množství 1 až 5 g-molekul na 1 g-sbom promotujícího kovu a úpravou pH na 7 až 8 přídavkem hydroxidu amonného ták, že se roztok, popřípadě s přídavkem inertního nosiče zahustí do konzistence aikrokrystalická pasty s-óbaaham 15 až 50 B hmotnostních vlhkosti, ■pasta se suší a zároveň kalcinuje v kontinuální míchané suěárně v proudu spalin plynového hořáku a/nebo vzduchu při teplotě 250 až 350 "C, zíkaný prach s* smísí s tabletačními přísadami, popřípadě se přidá uhličitan amonný v množství až 40 B hmotnostnícha směs se tvaruje do tvaru tablet, které se výžíhají za přístupu vzduchu oři teplotě 300 až 400 eC po dobu 5 až 24 hodin. Metoda umožňuje reprodukovatelnost podmínek jednotlivých výrobních operací v průmyslovém měřítku.A method for producing multicomponent catalysts for the oxidation of aldehydes to carboxylic acids by mixing a homogeneous aqueous solution of the starting compounds of the active components, which are oxides of molybdenum, vanadium and other promoting metals from I., V. and VIII. of the Mendeleev periodic system, which determines the atomic ratio of molybdenum to vanadium from 2:1 to 12:1 and the atomic ratio of promoters to molybdenum from 0.01 to 0.5 with organic hydroxy acids selected from the group including tartaric and citric acid in an amount of 1 to 5 g-molecules per 1 g-molecule of the promoting metal and adjusting the pH to 7 to 8 by adding ammonium hydroxide so that the solution, optionally with the addition of an inert carrier, is concentrated to the consistency of a microcrystalline paste with a moisture content of 15 to 50% by weight, the paste is dried and simultaneously calcined in a continuous stirred kiln in the flow of flue gases of a gas burner and/or air at a temperature of 250 to 350°C, the obtained powder is mixed with tableting additives, optionally ammonium carbonate is added in an amount of up to 40 B by weight and the mixture is shaped into tablets which are annealed in the presence of air at a temperature of 300 to 400 eC for 5 to 24 hours. The method allows the reproducibility of the conditions of individual production operations on an industrial scale.

Description

Vynález se týká způsobu výroby vícesložkových katalyzátorů pro oxidaci aldehydů na karboxylové kyaellny v plynná fázi.The invention relates to a method for producing multicomponent catalysts for the oxidation of aldehydes to carboxylic acids in the gas phase.

Pro katalytickou ioxidaci aldehydů jako je například akrolein nebo natakrolaia na odpovídající karboxylové kyseliny to je na kyselinu akrylovou nebo metakrylovou se běžně používají vícesložkové katalyzátory na bázi směsných oxidů molybdenu, vanadu a dalších promotujících kovů z I., V. a VIII. skupiny Mendělejevová periodického systému.For the catalytic oxidation of aldehydes such as acrolein or natacrolia to the corresponding carboxylic acids, i.e. acrylic or methacrylic acid, multicomponent catalysts based on mixed oxides of molybdenum, vanadium and other promoting metals from groups I, V and VIII of the Mendeleev periodic system are commonly used.

Základním nedostatkem věech dosud známých postupů přípravy katalyzátorů tohoto typu je Spatná reprodukovatelnost podmínek jednotlivých výrobních operaci v průmyslovém měřítku vedoucí k rozdílným katalytickým vlastnostem jednotlivých šarěí katalyzátorů.The basic shortcoming of all previously known processes for preparing catalysts of this type is the poor reproducibility of the conditions of individual production operations on an industrial scale, leading to different catalytic properties of individual batches of catalysts.

Tyto vícesložkové katalyzátory se připravují nejěastěji srážením z roztoků rozpustných sloučenin aktivních složek a to za přítomnosti nosiče nebo bez něho. Po odpaření vody se získané hmota dále tepelně zpracovává, obsažené soli se termicky rozloží, směs se vytvaruje a vyžíhá, čímž získá požadované katalytické vlastnosti.These multicomponent catalysts are most often prepared by precipitation from solutions of soluble compounds of the active components, in the presence or absence of a carrier. After evaporation of water, the obtained mass is further thermally treated, the contained salts are thermally decomposed, the mixture is shaped and calcined, thereby obtaining the desired catalytic properties.

Základní nevýhodou nejčastěji používaná arážeoí aetody je velká citlivost složení vznikající sraženiny na pořadí aíaenl roztoků, rychlosti dávkováni, koncentraci roztoků a na pH prostředí. ·The main disadvantage of the most commonly used precipitation method is the high sensitivity of the composition of the resulting precipitate to the order of the aqueous solutions, the dosing rate, the concentration of the solutions and the pH of the environment.

Udržet konstantní a reprodukovatelné podmínky srážení je u mnohosložkového systému velmi obtížné a tato okolnost je jednou z příčin nehomogenity složení jednotlivých ěarší při přípravě katalyzátoru v průmyslovém měřítku.Maintaining constant and reproducible precipitation conditions is very difficult in a multicomponent system, and this circumstance is one of the causes of the inhomogeneity of the composition of individual layers during the preparation of the catalyst on an industrial scale.

Značný pokrok v tomto směru přináší použití koaplexotvorných činidel, jak je uvedeno v čs. AO č. 188 414, zaručující udržení všech složek kstalizétorů v homogenním roztoku až do stadia jeho zahuštění do mikrokrystalická pasty. Uvedené AO však stejně jako jiné až dosud známé postupy neřeší dostatečným způsobem vyhovující postup dalšího tepelného .zpracování zahuštěné suspenze (pasty) v průmyslových podmínkách.Considerable progress in this direction is brought by the use of coaplexing agents, as stated in Czech Patent Application No. 188 414, which guarantees the maintenance of all components of the catalysts in a homogeneous solution until the stage of its thickening into a microcrystalline paste. However, the aforementioned Patent Application, like other previously known procedures, does not sufficiently address the satisfactory procedure for further thermal processing of the thickened suspension (paste) in industrial conditions.

Výchozími surovinami pro přípravu katalyzátorů pro oxidaci 'aldehydů jsou nejSastšji heptamolybdenan hexaaraonný, vanadičnan amonný a dusičnany ostatních promotujících kovů. Vedlejším produktem vznikajícím při smísení jejich vodných roztoků|je proto dusičnan amonný, který je příčinou značných obtíží při jejich dalším termickém zpracování.The starting materials for the preparation of catalysts for the oxidation of aldehydes are most often hexaammonium heptamolybdate, ammonium vanadate and nitrates of other promoting metals. The by-product formed when mixing their aqueous solutions is therefore ammonium nitrate, which causes considerable difficulties in their further thermal processing.

Tepelný rozklad dusičnanu amonného je pochod silně exothermní, který zaj přítomnosti solí kovů probíhá autokatalyticky. Teplo uvolněná při tomto rojtkladu může snadno zvýšit teplotu na hranici, kdy se rozklad stává již nezvládnutelným a katalyzátoru v této fázi hrozí nebezpečí nadměrného přehřátí, které je pak příčinnou ztráty jeho dobrých katalytických vlastností.The thermal decomposition of ammonium nitrate is a strongly exothermic process, which in the presence of metal salts proceeds autocatalytically. The heat released during this decomposition can easily increase the temperature to the point where the decomposition becomes unmanageable and the catalyst at this stage is at risk of excessive overheating, which then causes the loss of its good catalytic properties.

Přítomnost komplexotvorných látek toto nebezpečí ještě dále zvyšuje a posouvá počátek termického rozkladu NH^NOj do oblasti nižších teplot. Operace sušení a kaleinace (termického rozkladu solí) je z tohoto hlediska vysoce náročnou operací, která vyžaduje odpovídající technologické zařízení.The presence of complexing agents further increases this danger and shifts the onset of thermal decomposition of NH^NOj to the lower temperature range. The drying and calcination operation (thermal decomposition of salts) is from this point of view a highly demanding operation that requires appropriate technological equipment.

Uskutečnění této opsracs z* podmínek uvedených v AO 188 414 je možné pouze v laboratorním měřítku, kdy lze zaručit poměrně dobrý odvod tepla ze sušené a kalcinované hmoty. Rovněž další postup zpracování katalyzátorové hmoty uvedený v tomto AO je pro větší měřítko nevhodný, nebol navržené žíhání katalyzátoru v préškovité formě působí redukci spodních vrstev materiálu a je opět uskutečnitelné pouze v malém laboratorním mšřítku, kde lze zaručit dostatečný přístup vzduchu k celé vsázce žíhaného katalyzátoru.The implementation of this operation under the conditions specified in AO 188 414 is only possible on a laboratory scale, where relatively good heat removal from the dried and calcined mass can be guaranteed. Also, the further process of processing the catalyst mass specified in this AO is unsuitable for a larger scale, because the proposed annealing of the catalyst in powder form causes a reduction of the lower layers of the material and is again feasible only in a small laboratory scale, where sufficient air access to the entire batch of annealed catalyst can be guaranteed.

Pokrok ve srovnání se způsobem výroby katalyzátoru podle čs. AO č. 188 414 spočívá nejen ve zvýšení výtěžku užitečných produktů oxidace aldehydů o cca-3 %, jak dokládá tabulka I, zejména však ve skutečnosti, že postup podle tohoto vynálezu je realizovatelný v průmyslovém měřítku, zatímco postup přípravy katalyzátoru podle čs. A0 č. 188 414 lze realizovat pouze v malém laboratorním zařízení.The progress compared to the method of producing a catalyst according to Czechoslovak Patent Application No. 188,414 consists not only in the increase in the yield of useful products of aldehyde oxidation by approximately 3%, as shown in Table I, but especially in the fact that the process according to the present invention is feasible on an industrial scale, while the process of preparing a catalyst according to Czechoslovak Patent Application No. 188,414 can only be implemented in a small laboratory facility.

Podstata způsobu výroby vícesložkových katalyzátorů pro oxidaci aldehydů na karboxylové kyseliny smísením homogenního vodného roatoku výchozích sloučenin aktivních složek, kterými jsou oxidy molybdenu, vanadu a dalších promotujících kovů z I., V. a VIII. skupiny Mendělejevová periodického systému, přičemž atomární poměr molybdenu ku vanadu je 0,01 až 0,5 s organickými hydroxykyselinami zvolenými ze skupiny zahrnující kyselinu vinnou a citrónovou v .množství 1 až 5 g-molekul na 1 g-atom promotujícího kovu a úpravou pH na 7 až 8 přídavkem hydroxydu amonného spočívá podle vynálezu v tom, že se roztok, popřípadě s přídavkem inertního nosiče zahustí do konzistence mikrokrystalické pasty s obsahem 15 až 50 % hmotnostních vlhkosti, pasta se suší a zároveň kalcinuje v kontinuální míchané sušárně v proudu spalin plynového hořáku a/nebo vzduchu při teplotě 250 až 350 °C, získaný prach se smísí s tahletačnínji přísadami, popřípadě se přidá uhličitan amonný v množství až 40 % hmotnostních a směs se tvaruje do tvaru tablet, které se vyžíhají za přístupu vzduchu při teplotě 300 až 400 °C po dobu 5 až 24 hodin. Výhodný tvar tablet jsou rovnostranné válečky rozměru 4 až 6 mm nejlépe s otvorem uprostřed.The essence of the method for producing multicomponent catalysts for the oxidation of aldehydes to carboxylic acids by mixing a homogeneous aqueous stream of starting compounds of active components, which are oxides of molybdenum, vanadium and other promoting metals from I., V. and VIII. of the Mendeleev group of the periodic system, the atomic ratio of molybdenum to vanadium being 0.01 to 0.5 with organic hydroxy acids selected from the group comprising tartaric and citric acid in an amount of 1 to 5 g-molecules per 1 g-atom of the promoting metal and adjusting the pH to 7 to 8 by adding ammonium hydroxide, according to the invention, the solution, optionally with the addition of an inert carrier, is concentrated to the consistency of a microcrystalline paste with a moisture content of 15 to 50% by weight, the paste is dried and simultaneously calcined in a continuous stirred dryer in the flow of flue gases of a gas burner and/or air at a temperature of 250 to 350 °C, the obtained powder is mixed with tableting additives, optionally ammonium carbonate is added in an amount of up to 40% by weight and the mixture is shaped into tablets, which are annealed in the presence of air at a temperature 300 to 400 °C for 5 to 24 hours. The preferred shape of the tablets is equilateral cylinders measuring 4 to 6 mm, preferably with a hole in the middle.

Uvedený půstup přípravy vícesložkových katalyzátorů pro oxidaci aldehydů zaručuje výborné katalytické vlastnosti katalyzátorů a dokonalou homogenitu jejich jednotlivých šarží z následujících důvodů:The above-mentioned approach to the preparation of multicomponent catalysts for the oxidation of aldehydes guarantees excellent catalytic properties of the catalysts and perfect homogeneity of their individual batches for the following reasons:

1. Použití kombinace hydroxykyseliny a KH^OH zaručuje udržení polykomponentní směsi aktivních složek v roztoku až do stádia zahuštění na pastu s požadovaným obsahem vlhkosti, čímž se dosahuje dokonalé homogenity směsi.1. The use of a combination of hydroxy acid and KH^OH guarantees the maintenance of the polycomponent mixture of active ingredients in solution until the stage of thickening into a paste with the desired moisture content, thereby achieving perfect homogeneity of the mixture.

2. Vhodné spojení ertdotermního sušení a exothermní kalcinace za použití kontinuální míchané sušárny s plynným sušícím médiem zajištuje dokonalou regulaci teploty, kdy teplotu sušárny lze regulovat v požadovaných mezích volbou obsahu vlhkosti v pastě, rychlostí dávkování pasty do sušárny, volbou teploty pláště sušárny i vstupní teplotou plynného sušícího media, což vylučuje možnost nežádoucího přehřátí katalyzátoru.2. A suitable combination of ertdothermal drying and exothermic calcination using a continuous stirred dryer with a gaseous drying medium ensures perfect temperature control, where the temperature of the dryer can be regulated within the required limits by selecting the moisture content in the paste, the rate of dosing the paste into the dryer, the temperature of the dryer jacket and the inlet temperature of the gaseous drying medium, which eliminates the possibility of undesirable overheating of the catalyst.

3. Snadné udržení konstantních podmínek pracovního režimu základních operací výroby katalyzátorů pak zaručuje dokonalou homogenitu a reprodukovatelnost výroby katalyzátorů v libovolném množství.3. Easy maintenance of constant operating conditions of the basic operations of catalyst production guarantees perfect homogeneity and reproducibility of catalyst production in any quantity.

4. Případným přídavkem uhličitanu amonného před tabletací lze pak déle vhodně ovlivnit tvorbu makroporésní struktury katalyzátoru a tak eliminovat negativní vliv vnitřní difúze na selektivitu oxidační reakce.4. By optionally adding ammonium carbonate before tableting, the formation of the macroporous structure of the catalyst can be suitably influenced for a longer period of time and thus eliminate the negative effect of internal diffusion on the selectivity of the oxidation reaction.

5. Tvarováním katalyzátoru do tvaru válečků s vnitřním otvorem lže pak zaručit lepěí využití vnitřního povrchu katalyzátoru, snížit náklady na suroviny při jeho výrobě a zlepšit hydrodynamické podmínky v reaktoru.5. By shaping the catalyst into the shape of cylinders with an internal hole, it is possible to guarantee better use of the internal surface of the catalyst, reduce the cost of raw materials in its production and improve the hydrodynamic conditions in the reactor.

Katalyzátory vyrobené podle tohoto vynálezu se vyznačují při oxidaci aldehydů vysokou aktivitou a selektivitou. S výhodou mohou být použity pro druhý oxidační stupeň v procesu výroby kyseliny akrylové z propenu.The catalysts produced according to the present invention are characterized by high activity and selectivity in the oxidation of aldehydes. They can be advantageously used for the second oxidation step in the process of producing acrylic acid from propene.

Katalyzátor připravený podle tohoto vynálezu při použiti pro oxidaci akroleinu na kyselinu akrylovou poskytuje za stejných podmínek vyšší výtěžky kyseliny akrylové než katalyzátoru shodného složení připravený v laboratorním měřítku podle č. AO č. 188 414 jak dokládá následující tabulka I.The catalyst prepared according to this invention, when used for the oxidation of acrolein to acrylic acid, provides, under the same conditions, higher yields of acrylic acid than the catalyst of the same composition prepared on a laboratory scale according to AO No. 188,414, as shown in the following Table I.

Tabulka S. ITable S.I

Katalyzátor dle AO 188 414 Catalyst according to AO 188 414 Katalyzátor dle tohoto vynálezu Catalyst according to this invention konverze akroleinu acrolein conversion 95 % 95% 100 % 100% výtěžek kyseliny acid yield akrylové acrylic 92 % 92% 95 % 95%

Vlastní postup přípravy katalyzátoru podle tohoto vynálezu je dále objasněn následujícím ' příkladem:The actual process of preparing the catalyst according to the present invention is further illustrated by the following example:

PřikladlExample

Postupně se připraví:Gradually prepare:

Roztok A 1 - v 132 1 vody se rozpustí 28 kg heptamolybdenanu hyxaamonného a přidá se 7,2 1 26% hydroxidu amonnéhoSolution A 1 - 28 kg of hexaammonium heptamolybdate is dissolved in 132 l of water and 7.2 l of 26% ammonium hydroxide is added

Roztok A 2 - v 222 1 vody se rozpustí 4,6 kg vanadičnanu amonnéhoSolution A 2 - 4.6 kg of ammonium vanadate is dissolved in 222 l of water

Roztok B 1 - v 43 1 vody se rozpustí 8 kg kyseliny vinné a 6,4 kg dusičnanu měSnatéhoSolution B 1 - 8 kg of tartaric acid and 6.4 kg of potassium nitrate are dissolved in 43 l of water.

Roztok B 2 - v 32 1 vody se rozpustí 3 kg kyseliny vinné a 2,7 kg dusičnanu Selezitého.Solution B 2 - 3 kg of tartaric acid and 2.7 kg of Selezite nitrate are dissolved in 32 1 of water.

Slitím roztoků A 1 a A 2 vznikne roztok A. Slitím roztoků B 1 a B 2 vznikne roztok B.Combining solutions A 1 and A 2 produces solution A. Combining solutions B 1 and B 2 produces solution B.

Po jejích smíchání se upraví pH pomocí Jiydroxidu amonného na hodnotu 7,3. Výsledný homogenní roztok se zahuštuje při 80 až 100 °C na pastu s minimálním obsahem vlhkosti 15% hmot. Pasta se současně buší a kalcinuje v kontinuální míchané suěárně v proudu vzduchu a spalin zemního plynu za následujících podmínek: množství vzduchu procházející sušárnou - 70 až 75 kg/h, teplota na výstupu suěárny + 300 °C, spotřeba senního plynu 2,5 m^/h, teplote tempemečního pláště sušárny * 240 °C.After mixing, the pH is adjusted to 7.3 with ammonium hydroxide. The resulting homogeneous solution is concentrated at 80 to 100 °C to a paste with a minimum moisture content of 15% by weight. The paste is simultaneously pounded and calcined in a continuous stirred kiln in a stream of air and natural gas flue gases under the following conditions: amount of air passing through the kiln - 70 to 75 kg/h, temperature at the kiln outlet + 300 °C, hay gas consumption 2.5 m^/h, temperature of the kiln jacket * 240 °C.

Prach katalyzátoru se po přidání grafitu a kaolinu a 10 kg uhličitanu amonného tabletuje do tvaru válečků 6 x 3 mm s vnitřním otvorem o průměru 2 mm a nakonec se žíhá v peci za přístupu vzduchu a to 5 hodin při 300 °C a 10 hodin při 350 °C.After adding graphite and kaolin and 10 kg of ammonium carbonate, the catalyst dust is tableted into the shape of 6 x 3 mm cylinders with an internal hole of 2 mm diameter and finally annealed in an oven with air access for 5 hours at 300 °C and 10 hours at 350 °C.

Claims (1)

Způsob výroby vícesložkových katalyzátorů pro oxidaci aldehydů na karboxylové kyseliny smísením homogenního vodného roztoku výchozích sloučenin aktivních složek, kterými jsou oxidy molybdenu, vanadu a dalších promotujících kovů z I., V. a Vili. skupiny Mendělejevova periodického systému, přičemž atomární poměr molybdenu ku vendanu je 2 : 1 až 12 : 1 a atomární poměr promotorů ku molybdenu je 0,01 až 0,5 s organickými hydroxykyselinami zvolenými ze skupiny zahrnující kyselinu vinnou a citrónovou v množství 1 až 5 g-molekul nelg-etom promotujícího kovu a úpravou pH na 7 až 8 přídavkem hydroxidu amonného, vyznačený tím, že ee rostok, popřípadě e přídavkem inertního noeiče sehuetí do koneietenoe mlkrokryeialioká pasty s obsahem 15 až 50 % hmotnostních vlhkosti, pasta se suší |e zároveň kalcinuje v kontinuální míchané sušárně v proudu spalin plynového hořáku a/nebo vzduchu při teplotě 250 až 350 °C, získaný prach se smísí s tabletačními přísadami, poořípadě se přidá uhličitan amonný v množství až 40 % hmotnostních a směs se tvaruje do tvaru tablet, která ee vytahají se přístupu vsduehu při teplotě 300 až 400 °C po dobu 5 až 24 hodin.A process for the preparation of multi-component catalysts for the oxidation of aldehydes to carboxylic acids by mixing a homogeneous aqueous solution of the starting compounds of the active ingredients, which are the oxides of molybdenum, vanadium and other promoting metals of I., V. and VII. of the Mendeleyev periodic system, wherein the atomic ratio of molybdenum to vendan is 2: 1 to 12: 1 and the atomic ratio of promoters to molybdenum is 0.01 to 0.5 with organic hydroxy acids selected from the group comprising tartaric and citric acid in an amount of 1-5 g - a non-lg-etoma-promoting metal molecule and adjusting the pH to 7-8 by addition of ammonium hydroxide, characterized in that the rostok, optionally by addition of an inert carrier, is dried into a microcrystalline paste having a moisture content of 15-50% by weight; calcined in a continuous stirred drier in a flue gas stream of gas burner and / or air at a temperature of 250 to 350 ° C, the dust obtained is mixed with tableting ingredients, optionally up to 40% by weight of ammonium carbonate and formed into tablets which ee are pulled out of the access at 300 to 400 ° C for 5 to 24 hours.
CS847075A 1984-09-20 1984-09-20 Process for the production of multi-component catalysts for the oxidation of aldehydes CS244033B1 (en)