CS249477B1 - A method of casting the raffinone ferochrome - Google Patents

A method of casting the raffinone ferochrome Download PDF

Info

Publication number
CS249477B1
CS249477B1 CS540685A CS540685A CS249477B1 CS 249477 B1 CS249477 B1 CS 249477B1 CS 540685 A CS540685 A CS 540685A CS 540685 A CS540685 A CS 540685A CS 249477 B1 CS249477 B1 CS 249477B1
Authority
CS
Czechoslovakia
Prior art keywords
casting
block
sand
ferro
chromium
Prior art date
Application number
CS540685A
Other languages
Czech (cs)
Slovak (sk)
Inventor
Arnost Borak
Stefan Svorencik
Andrej Krivda
Original Assignee
Arnost Borak
Stefan Svorencik
Andrej Krivda
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Arnost Borak, Stefan Svorencik, Andrej Krivda filed Critical Arnost Borak
Priority to CS540685A priority Critical patent/CS249477B1/en
Publication of CS249477B1 publication Critical patent/CS249477B1/en

Abstract

Riešenie sa týká spósobu odllevania rafinač- ného ferochómu. Ferochřóm sa odlieva na pieskové ložko, udržiavané na troskovom bloku, pričom pieskové ložko tvoři 15-ti vrstva piesku. Podlá riešenia blok ferochromu sa z lóžka vyberie po stuhnutí, keď jeho povrchová teplota je 900 až 1 050 °C.The solution concerns a method of casting refined ferrochrome. The ferrochrome is cast on a sand bed, maintained on a slag block, the sand bed being formed by 15 layers of sand. According to the solution, the ferrochrome block is removed from the bed after solidification, when its surface temperature is 900 to 1,050 °C.

Description

Vynález sa týká spósobu odlievania nízko a stredne uhlíkatého ferochrómu.The invention relates to a process for casting low and medium carbon ferro-chromium.

Rafinačný ferochróm sa v súčasnosti odlieva prevážne do oceloliatinové kokily. Sú známe tiež spósoby odlievania do kovových foriem, ktoré sú chráněné žiaruvzdorným materiálom, ako napr. vymurovaním šamotovými tehlami, otroskovaním, vypieskovaním alebo odlievanie do formy uloženej na hruběj vrstvě plesku.At present, the ferro-chromium is cast mainly into a cast iron mold. Methods of casting into metal molds which are protected by a refractory material, such as e.g. by fireclay bricks, sandblasting, sandblasting or casting into a mold deposited on a thick layer of the ball.

Nevýhodou postupu odlievania do oceloliatinové kokily sú vysoké prevádzkové náklady. Pri postupoch odlievania, kde spodnú časť liaceho miesta tvoří hrubá vrstva piesku, sa ferochróm znečisťuje pripečeninami piesku a vzniká nevhodný tvar bloku ferochrómu pre ďalšie spracovanieA disadvantage of the casting process in a cast iron mold is the high operating costs. In casting processes, where the bottom of the casting site is formed by a thick layer of sand, ferro-chromium is contaminated by sand deposits and an inappropriate shape of the ferro-chromium block for further processing

Uvedené nedostatky odstraňuje spósob odlievania rafinačného ferochrómu na pieskové lóžko, ktoré sa udržiava na troskovom bloku, pričom pieskové lóžko tvoři vrstva piesku vo vymedzenom rozmedzí 3 až 15 cm. Podstata vynálezu spočívá v tom, že blok ferochrómu sa vyberá po stuhnutí, keď jeho povrchová teplota je 900 až 1 050 °C.These drawbacks are eliminated by the method of casting the refinery ferrochrome onto a sand bed, which is maintained on the slag block, the sand bed forming a sand layer in the defined range of 3 to 15 cm. The essence of the invention is that the ferrochromic block is removed after solidification when its surface temperature is 900 to 1050 ° C.

Liace miesto sa obvykle skládá z kovověj formy, v ktorej sa připraví troškový blok, na ktorom sa udržuje pieskové lóžko. Troškový blok o hrúbke na 15 cm sa připraví z dostupnéj, tepelne stálej trosky.The casting site usually consists of a metal mold in which a tiny block is prepared on which a sand bed is maintained. A tiny block of 15 cm thickness is prepared from an available, thermally stable slag.

Hrúbka vrstvy piesku, udržiavaná na troskovom bloku, je závislá na kvalitě odlievaného rafinačného ferochrómu, na obsah uhlíka, pričom pri odlievaní nízkouhlíkatého sa udržuje vrstva piesku na dolnej hranici a postupné so zvyšováním obsahu uhlíka v kove sa jej vrstva zvyšuje až na hornú hranicu.The thickness of the sand layer maintained on the slag block is dependent on the quality of the casting refinery ferrochrome, the carbon content, while the low carbon casting keeps the sand layer at the lower boundary and gradually increases to the upper boundary as the carbon content in the metal increases.

Výhodou postupu podlá vynálezu sú nízké prevádzkové náklady na odlievanie a zvýšenie čistoty ferochrómu. K príprave liaceho miesta sa používá jednoduché a lahko dostupné zariadenie a materiál. Například na přípravu troškového bloku sa móže použíť troska, ktorá tvoří odpad z výroby ferozliatin.The advantage of the process according to the invention is the low operating costs for casting and increasing the purity of ferrochromium. Simple and readily available equipment and materials are used to prepare the casting site. For example, a slag may be used to prepare the tiny block, which constitutes waste from the production of ferroalloys.

Odlievacie zariadenie po vybratí ferochrómu a doplnění pieskom je připravené na ďalšie liatie a jeho životnost je dlhodobá. Pri poškodení je lahko obnovitelné. Zvýšená čistota kovu je zaistená dodržanim teploty vyberaného bloku kovu z lóžka, tj. v čase, keď pieskové lóžko je ešte rnákké až tekuté, čím sa zaisťuje jeho dobré oddelenie od ferochrómu.The casting device is ready for further casting after removal of ferro-chromium and refilling with sand and its service life is long-lasting. Damage is easily recoverable. Increased metal purity is ensured by maintaining the temperature of the selected metal block from the bed, i. at a time when the sand bed is still fluid to liquid, ensuring its good separation from ferrochromium.

Postup podlá vynálezu je ralizovaný pri odlievaní ferochrómu s obsahom uhlíka 0,06 až 0,15 %.The process according to the invention is ralized in a ferro-chromium casting with a carbon content of 0.06 to 0.15%.

Kovová forma - rám s dnom o rozmerooh 140 x 240 cm, výška 50 cm, smerom nahor rozšířený. Do kovového rámu sa naleje tekutá troska z výroby ferochrómu uhlíkatého o hrúbke cca 15 cm.Metal mold - frame with bottom dimensions 140 x 240 cm, height 50 cm, extended upwards. A liquid slag from the production of carbon ferro-chromium of about 15 cm thickness is poured into the metal frame.

Po stuhnuti sa na troskovom bloku připraví pieskové lóžko nasypáním a urovnáním vrstvy piesku o hrúbke 4 cm.After solidification, a sand bed is prepared on the slag block by pouring and leveling a 4 cm thick sand layer.

Takto je liace zariadenie připravené k odlievaniu ferochrómu a ich počet je závislý na množstve odlievaného ferochrómu, tj. pre odlievanie 6 t ferochrómu stačia 3 ks.Thus, the casting device is ready for casting of ferrochromium and its number depends on the amount of ferrochromium being cast, ie. For casting 6 t of ferrochromium, 3 pieces are sufficient.

Po dosiahnutí povrchovej teploty bloku ferochrómu 1 000 °C sa ferochróm z lóžka vyberie, pričom merítkom správnosti postupu je, že pieskové lóžko zo spodnej strany bloku ferochrómu sa oddělí a zostane na troskovom bloku v miikkom až tekutom stave. Po doplnění vrstvy piesku na požadovaná výšku je liace zariadenie připravené k ďalšiemu liatiu.Once the surface temperature of the ferro-chromium block has reached 1000 ° C, the ferro-chromium is removed from the bed, and the measure of correctness is that the sand bed from the underside of the ferro-chromium block is separated and remains on the slag block in a mild to liquid state. After the sand layer has been filled to the desired height, the casting machine is ready for further casting.

Claims (1)

PREDMET V YNALEZUOBJECT IN YNALEZ Spósob odlievania ferochrómu rafinačného na pieskové lóžko udržiavané na troskovom bloku, pričom pieskové lóžko tvoří vrstva piesku 3 až 15 cm, vyznačujúci sa tým, ža blok ferochrómu sa vyberá po stuhnuti, keď jeho povrchová teplota je 900 až 1 050 °C.A method of casting a ferro-chromium refined sand bed maintained on a slag block, the sand bed forming a sand layer of 3-15 cm, characterized in that the ferrochromium block is removed after solidification when its surface temperature is 900 to 1050 ° C.
CS540685A 1985-07-23 1985-07-23 A method of casting the raffinone ferochrome CS249477B1 (en)