CS253371B1 - Method of non-destructive determination of residual life of metallic materials - Google Patents

Method of non-destructive determination of residual life of metallic materials Download PDF

Info

Publication number
CS253371B1
CS253371B1 CS85834A CS83485A CS253371B1 CS 253371 B1 CS253371 B1 CS 253371B1 CS 85834 A CS85834 A CS 85834A CS 83485 A CS83485 A CS 83485A CS 253371 B1 CS253371 B1 CS 253371B1
Authority
CS
Czechoslovakia
Prior art keywords
damage
parts
determined
examined
component
Prior art date
Application number
CS85834A
Other languages
Czech (cs)
Other versions
CS83485A1 (en
Inventor
Ivan Otevrel
Vaclav Sklenicka
Original Assignee
Ivan Otevrel
Vaclav Sklenicka
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Ivan Otevrel, Vaclav Sklenicka filed Critical Ivan Otevrel
Priority to CS85834A priority Critical patent/CS253371B1/en
Publication of CS83485A1 publication Critical patent/CS83485A1/en
Publication of CS253371B1 publication Critical patent/CS253371B1/en

Abstract

Nový postup je založen na mikrostrukturní analýze místa poškození a spočívá v následujícím: u vyšetřovaného dílce, popřípadě sopboru dílců se zjistí jejich kritické místo, určí se mezní hodnota poškození použitého kovového^materiálu a stanoví se závislost poškození povrchové hladiny dílců na jejich celkovém poškození, načež se po předem stanovené době provozu u jednotlivých vyšetřovaných dílců provede metalografický výbrus dílce v kritickém místě a metalograficky se vyhodnotí stupeň poškození povrchové hladiny dílců, přičemž se ze stupně zjištěného poškození povrchové hladiny dílců vypočte celkové poškození dílce, načež se u každého ze souboru vyšetřovaných dílců nejméně jednou opakuje, přičemž se metalografický výbrus provede opět v kritickém místě dilců, a ze srovnání časově závislého nárůstů poškození dílců a předem určeného mezního poškození užitého materiálu se odvodí zbytková životnost materiálu dílců.The new procedure is based on microstructural analysis of the damage location and consists of the following: the critical location of the examined part or group of parts is determined, the limit value of damage to the metal material used is determined and the dependence of the damage to the surface of the parts on their total damage is determined, after which, after a predetermined period of operation, metallographic grinding of the part is performed in the critical location for the individual examined parts and the degree of damage to the surface of the parts is metallographically evaluated, while the total damage to the part is calculated from the degree of damage to the surface of the parts found, after which it is repeated at least once for each of the group of examined parts, while metallographic grinding is performed again in the critical location of the parts, and the residual service life of the part material is derived from the comparison of the time-dependent increase in damage to the parts and the predetermined limit damage to the material used.

Description

Vynález se týká nového způsobu nedestruktivního zjišťování zbytkové životnosti kovových materiálů u dílců dlouhodobě namáhaných vysokoteplotním creepem. Nový postup je založen, na použití mikrostrukturní analýzy a je vhodný zejména také pro stanovení zbytkové životnosti reakčnich trubek reformingových pecí, zhotovených z vysoce legovaných austenitických GrNi ocelí.The invention relates to a new method of non-destructive determination of the residual life of metallic materials in parts subjected to long-term high-temperature creep. The new procedure is based on the use of microstructural analysis and is particularly suitable for determining the residual life of reaction tubes of reforming furnaces made of high-alloy austenitic GrNi steels.

Současný trend rozvoje strojírenství preferuje maximální využití materiálu. Potřebného učinku se dociluje jednak vhodným dimezováním součástí, jednak kontrolovaným celkovým vyčerpáním limitujících vlastností materiálu. U zařízení, které je namáháno vysokoteplotním creepem, je přímo nezbytné počítat s postupnou degradací žárupevných vlastností materiálu a akceptovat v provozních podmínkách určité množství defektůoThe current trend in the development of mechanical engineering prefers maximum use of material. The necessary effect is achieved both by appropriate dimensioning of components and by controlled total exhaustion of limiting material properties. In equipment subjected to high-temperature creep, it is directly necessary to count on gradual degradation of refractory properties of the material and to accept a certain amount of defects under operating conditions.

Kovový materiál pracující dlouhodobé v oblastech vysokoteplotního creepu , kde pod pojmem creep (tečení) se rozumí časově závislá složka plastické deformace materiálu, ztrácí v důsledku mikro strukturních změn postupně své původní žárupevné vlastnosti.A metallic material operating for a long time in areas of high-temperature creep, where the term creep refers to the time-dependent component of the plastic deformation of the material, gradually loses its original refractory properties due to microstructural changes.

U takového materiálu dochází po absolvování nezbytných stadií poškození, tj. vzniku, růstu a spojování mikrodutin-kavit, k takřka bezdeformačnímu lomu. Tento jev byl sledován u odstředivě litých procesních trubek, vystavených dlčíhodobě sálavému teplu v radiačních komorách pecí pro výrobu čpavku metanolu či vodíku parním reformováním uhlovodíků. U těchto trubek docházelo k porušení stěny bez předchozího výrazného natečení materiálu. Byly proto hledány možnosti, jak nedestruktivním způsobem zjistit včas skutečný stav trubky a předejít tak havarijním stavím.In such a material, after completing the necessary stages of damage, i.e. the formation, growth and connection of microvoids-cavities, an almost deformation-free fracture occurs. This phenomenon was observed in centrifugally cast process tubes, exposed for a long time to radiant heat in the radiation chambers of furnaces for the production of ammonia, methanol or hydrogen by steam reforming of hydrocarbons. In these tubes, the wall was broken without prior significant material flow. Therefore, possibilities were sought to determine the actual condition of the tube in a timely manner in a non-destructive manner and thus prevent emergency situations.

Úspěšné aplikování ultrazvuku naráží v tomto případě na problémy s rozptylem ultrazvukových vln na hrubozrrmé, odstředivě lité struktuře a se zajištěním vhodného vazebného prostředí mezi povrchem trubky a sondou. Je známo, že bylo vyvinuto ultrazvukové zkušební zařízení, které šplhá vlastní silou po trubce a provádí automatická měření. Nejsou však známy praktické výsledky této metody, která prozatím nedošla širšího uplatnění·The successful application of ultrasound in this case encounters problems with the scattering of ultrasonic waves on the coarse-grained, centrifugally cast structure and with ensuring a suitable coupling environment between the pipe surface and the probe. It is known that an ultrasonic testing device has been developed that climbs the pipe under its own power and performs automatic measurements. However, the practical results of this method are not known, and it has not yet been widely used.

253 371253,371

Zkoušky prozařováním je možno provádět pouze tzv· “metodou přes dvě stěny, která však vykazuje menší citlivost na defekty typu trhlina. Navíc je tato metoda provázena známými problémy souvisejícími s manipulací s gama-zéřiěi a není zajistitelná ani stoprocentní kontrola trubek·Radiation tests can only be performed using the so-called “double-wall method”, which is less sensitive to crack-type defects. In addition, this method is accompanied by known problems related to gamma ray handling and 100% tube inspection cannot be ensured.

Byla rovněž ověřována možnoet zjistit vnitřní defekty elektroinduktivní metodou, při níž byly vnitřní creepové trhliny z vnějšího povrchu trubky indikovány pomocí speciálně vyvinutého přístroje· Postupovalo se přitom tak, že cívkou, vyvolávající střídavé magnetické pole, byl zmapován povrch vyšetřované oblasti, přičemž se měřil stupeň ovlivnění budicího pole cívky vířivými proudy indukovanými ve stěně trubky· Popsaná metoda nevyžaduje sice vazebné prostředí mezi sondou a zkoušeným povrchem, je však nezbytné, aby sonda přiléhala dobře k vyšetřovanému dílci či součásti· Provedené zkoušky nadto prokázaly, že výsledky měření nedovolují vždy jednoznačnou interpretaci stupně poškození·»The possibility of detecting internal defects by the electroinductive method was also verified, in which internal creep cracks from the outer surface of the pipe were indicated using a specially developed device. The procedure was that a coil inducing an alternating magnetic field mapped the surface of the examined area, while the degree of influence of the coil excitation field by eddy currents induced in the pipe wall was measured. Although the described method does not require a coupling medium between the probe and the tested surface, it is necessary that the probe adheres well to the examined part or component. The tests performed also showed that the measurement results do not always allow an unambiguous interpretation of the degree of damage.»

Základním společným nedostatkem popsaných metod je pak skutečnost, že jejich fyzikální podstata umožňuje zjistit jen značně vyvinuté creepové trhliny· Archivaci výsledků měření je možno nadto provádět jen u zkoušek, prozařováním, zatímco u ultrazvukových a elektroinduktivních metod je to obtížné· K přednostem těchto metod je sice možno počítat mobilnost použitých přístrojů a bezprost řední, okamžité vyhodnocení naměřených hodnot, na druhé straně všakvzhledem k tomu, že zkoušky odhalí až poškození odpovídající předlomovému stavu, kdy trhliny postihly již značnou část stěny trubky, vyžadují tyto metody značně krátké časové odstupy mezi jednotlivými kontrolními měřeními· Pouhé, na empirii založené kvalitativní posouzení stavu poškození, bez návaznosti výsledků na jeho časový rozvoj, nedává nadto možnost predikovat zbytkovou životnost dílce·The basic common shortcoming of the described methods is the fact that their physical nature allows only to detect significantly developed creep cracks. Furthermore, archiving of measurement results can only be carried out for tests, by irradiation, while this is difficult for ultrasonic and electroinductive methods. The advantages of these methods include the mobility of the devices used and the direct, immediate evaluation of the measured values. On the other hand, due to the fact that the tests only reveal damage corresponding to the pre-fracture state, when cracks have already affected a significant part of the pipe wall, these methods require very short time intervals between individual control measurements. Furthermore, a mere, empirically based qualitative assessment of the state of damage, without linking the results to its development over time, does not allow predicting the residual service life of the part.

Popsané nedostaky dosud užívaných nedestruktivních zkušebních metod jsou naproti tomu odstraněny u způsobu nedestruktivního zjišťování zbytkové životnosti kovových materiálů u dílcůThe described shortcomings of the non-destructive testing methods used so far are, on the other hand, eliminated in the method of non-destructive determination of the residual service life of metal materials in parts.

- 3 253 371 dlouhodobě namáhaných vysokoteplotním creepem podle vynálezu, který je založen na mikrostrukturní analýze poškozeného místa a který spočívá v následujících krocích :- 3,253,371 long-term high-temperature creep stress according to the invention, which is based on microstructural analysis of the damaged area and which consists of the following steps:

a) u vyšetřovaného dílce, popřípadě souboru dílců se zjistí jejich kritické místo,a) the critical point of the examined component or set of components is determined,

b) určí se mezní hodnota poškození použitého kovového materiálu ab) the damage limit value of the metal material used is determined and

o) stanoví se závislost poškození povrchové hladiny dílců na jejich celkovém poškození, načež seo) the dependence of damage to the surface of the parts on their overall damage is determined, after which

d) po předem stanovené době provozu u jednotlivých vyšetřovaných dílců provede metalografický výbrus dílce v kritickém místě ad) after a predetermined period of operation for individual examined parts, metallographic grinding of the part at a critical point is performed and

e) metalograficky se vyhodnotí stupeň poškození povrchové hladiny dílců, přičemž see) the degree of damage to the surface of the parts is evaluated metallographically,

f) ze stupně zjištěného poškození povrchové hladiny dílců podle vztahu z bodu c)’ vypočte celkové poškození dílce, načež sef) from the degree of damage to the surface of the parts determined according to the relationship from point c)’, the total damage to the part is calculated, after which

g) postup podle bodů d) až f) u každého ze souboru vyšetřovaných dílců nejméně jednou opakuje, přičemž se metalografický výbrus. provede opět v kritickém místě dílců, ag) the procedure according to points d) to f) is repeated at least once for each of the set of examined parts, with the metallographic cutting being performed again at the critical point of the parts, and

h) ze srovnání časově závislého nárůstů poškození dílců a předem určeného mezního poškození užitého materiálu se odvodí zbytková životnost materiálu dílců.h) the residual service life of the component material is derived from a comparison of the time-dependent increase in component damage and the predetermined damage limit of the material used.

Postup podle vynálezu představuje v podstatě nový nedestruktivní apůsob zjišíování zbytkové životnosti creepově narušeného kovového materiálu, který je založen na poznatku, že z kvantifika ce poškození vnějšího povrchu vyšetřovaných dílců či souěástí lze odvodit poškození celkové· Opakovaným měřením je pak možno získat funkční závislost mezi poškozením dílce a dobou jeho reálného pro vozu, což umožní s vysokou pravděpodobností odhadnout další bezporuchový chod dílce, tzn· určit jeho zbytkovou životnost·The procedure according to the invention represents essentially a new non-destructive method of determining the residual life of a creep-damaged metallic material, which is based on the knowledge that the overall damage can be derived from the quantification of the damage to the outer surface of the examined parts or components. By repeated measurements, it is then possible to obtain a functional dependence between the damage to the part and the time of its real operation, which will allow to estimate with a high probability the further failure-free operation of the part, i.e. to determine its residual life.

Předností nového postupu, který je založen na použití mikrostrukturní analýzy, ve srovnání s dříve popsqnými metodáí^je kromě toho skutečnost, že mikrostrukturní analýzou je možno zjistit již velmi nízkou úroveň mezikrystalového poškození, což umožní předví·The advantage of the new procedure, which is based on the use of microstructural analysis, compared to previously described methods, is also the fact that microstructural analysis can detect even very low levels of intergranular damage, which will allow for the prediction of

253 371 dat zbytkovou životnost dílce či součásti s dostatečným předstihem·253,371 data the remaining life of a part or component well in advance

Uvažujeme-li nyní jednotlivé kroky postupu podle vynálezu samostatně, pak při stanovení kritického místa vyšetřovaného dílce či dílců je možno postupovat tak, žeIf we now consider the individual steps of the method according to the invention separately, then when determining the critical point of the examined part or parts, it is possible to proceed as follows:

- se buů vychází ze znalosti technologického procesu, který přímo předurčuje maximálně namáhané místo dílce, anebo- either based on knowledge of the technological process, which directly determines the maximum stressed area of the part, or

- ze znalosti předcházejících, pravidelně se v určitém místě dílce vyskytujících poruch, popřípadě- from knowledge of previous, regularly occurring defects in a certain part, or

- je možno provést detailní metalografické vyšetření stupně poškození jednotlivých částí reprezentativního dílce z vyšetřovaného souboru dílců, přičemž maximálně poškozenou oblast je možno považovat za kritickou·- it is possible to perform a detailed metallographic examination of the degree of damage to individual parts of a representative part from the examined set of parts, with the most damaged area being considered critical.

Stupeň poškození zkoušeného dílce se přitom určí pomocí některého ze známých kvantifikačních kriterií, kupříkladu z objemového podílu mezikrystalových dutin. Vyšetření 3e provede po předchozím odstranění provozem znehodnocené vrstvy·The degree of damage to the tested part is determined using one of the known quantification criteria, for example, the volume fraction of intercrystalline voids. Examination 3e is carried out after the layer damaged by operation has been removed.

Pro stanovení mezního poškození použitého kovového materiálu se nejméně jeden creepový vzorek materiálu, kupříkladu ve formě tyčky, vystaví podmínkám simulujícím provozní podmínky a to po dobu potřebnou k vyvolání lomu· Pomocí ^zvoleného kvantifikačního kriteriaftj· kupříkladu na základě podílu mezikrystalových dutin, se pak určí mezní poškození v činné oblasti vzorku, mimo oblast magistrální trhliny·To determine the limit damage of the metal material used, at least one creep sample of the material, for example in the form of a rod, is exposed to conditions simulating operational conditions for the time required to induce fracture. Using a selected quantification criterion, for example based on the proportion of intergranular voids, the limit damage is then determined in the active area of the sample, outside the area of the main crack.

V této souvislosti je třeba podotknout, že hodnota mezního poškození či porušení použitého kovového materiálu není v žádné souvislosti s kritickým místem či kritickou oblastí dílce· Číselná hodnota mezního poškození závisí pouze na zvoleném kvantifikačním kriteriu, popisujícím stav porušení materiálu, a platí vždy pro širokou skupinu materiálů obdobných vlastností®In this context, it should be noted that the value of the limit damage or failure of the metal material used is in no way related to the critical point or critical area of the part. The numerical value of the limit damage depends only on the selected quantification criterion describing the state of failure of the material, and is always valid for a wide group of materials with similar properties.

Postup odvození závislosti poškození povrchové hladiny dílců na jejich celkovém poškození, stejně jako postup zpracování metodiky zkoušení bude dále objasněn na konkrétním případě odstřeΜ *·The procedure for deriving the dependence of the damage to the surface of the parts on their total damage, as well as the procedure for developing the testing methodology, will be further explained using the specific case of a centrifuge *.

253 371 divě lité reformingové trubky 0 132x16, zhotovené z materiálu 40Cr2'5Ni20.253 371 cast reforming tubes 0 132x16, made of 40Cr2'5Ni20 material.

Creepové poškození, vyjádřené kupříkladu objemovým podílem mezikrystalových dutin, představuje důsledek nevyhnutéIného postupného procesu, který postihuje celou tloušťku stěny trubky. Je-li materiál vyšetřován ve fázi výskytu především ojedinělých kavit, je možno objemový podíl všech mezikrystalových dutin V nahradit objemovým podílem kavit V^ .Creep damage, expressed for example by the volume fraction of intercrystalline voids, is the result of an inevitable gradual process that affects the entire thickness of the tube wall. If the material is examined in the phase of occurrence of mainly isolated cavities, the volume fraction of all intercrystalline voids V can be replaced by the volume fraction of cavities V^ .

Každá hladina stěny trubky, tj. kružnice o poloměru r, kde rmin “ r * rmax ’ PřiSemž resp. rmax značí vnitřní, resp.Each surface of the pipe wall, i.e. a circle with radius r, where r min “ r * r max ' P řiSemž or r max denotes the inner, respectively.

vnější poloměr trubky, však vykažuje různý průběh poškození. Nestejné množství defektů se kromě toho jeví i v každém místě každé trubky radiačního systému pece, neboť ani vnější podmínky nejsou v celé peci konstantní a rozdílná je i odolnost materiálu proti tečení u jednotlivých trubek, které jsou navíc svařeny z většího počtu částí. Je proto nezbytné prověřovat, tak jako ostatně u všeóh metod, každou trubku individuálně.The outer radius of the tube, however, shows a different course of damage. In addition, an unequal number of defects also appears in each location of each tube of the furnace radiation system, because the external conditions are not constant throughout the furnace and the creep resistance of the material is also different for individual tubes, which are also welded from a larger number of parts. It is therefore necessary to check, as with all methods, each tube individually.

V souvislosti.s teplotou paroplynné směsi protékající trubkou, koeficienty přestupu tepla a dalšími podmínkami, má trubka své kritické oblasti či místa. Tato místa je možno zjistit, jak |již bylo dříve uvedeno, kupříkladu zdokumentováním již prasklých trubek anebo detailní mikrostrukturní analýzou trubky sledované reformingové pece.In connection with the temperature of the steam-gas mixture flowing through the tube, the heat transfer coefficients and other conditions, the tube has its critical areas or locations. These locations can be determined, as previously stated, for example by documenting already cracked tubes or by detailed microstructural analysis of the tube of the reforming furnace under study.

Poškození jednotlivých hladin trubky se mění spojitě, jestliže existuje kontinuita jak vnějších podmínek, tak i vlastností materiálu. Z poškození libovolné hladiny V^ je pak možno odvodit poškození celého průřezu stěny trubky vke· Tuto závislost lze vyjádřit vztahem vke ’ f <vki ) « kde f znamená funkce.The damage to individual pipe surfaces varies continuously if there is continuity of both external conditions and material properties. From the damage to any surface V^, it is then possible to derive the damage to the entire cross-section of the pipe wall v ke. This dependence can be expressed by the relation v ke ' f < v ki ) « where f means a function.

Hodnota objemového podílu kavit libovolné hladiny Vk£ se vypoč te pomoci vztahů publikovaných ve Studii ČSAV č. 8/77 Mezikrystalo vý lom při vysokoteplotním creepu kovů a slitin” autorů Skleničky,The value of the volume fraction of cavities of any surface V k £ is calculated using the relations published in the Study of the Czechoslovak Academy of Sciences No. 8/77 "Intercrystalline fracture during high-temperature creep of metals and alloys" by the authors Sklenička,

253 371253,371

Saxla, Čadka - Academia 1977 í 2Saxla, Čadka - Academia 1977 í 2

V· kiV·ki

V · ai /-/ kde Ngi jeV · a i /-/ where N gi is

plošná hustota výskytu mezikrystalových (mezidentritických) kavit, střední hodnota průměru kavit .areal density of occurrence of intercrystalline (interdendritic) cavities, mean value of cavity diameter.

Hodnoty N · a ď. se získají z následujících vztahů : SX X Nsi = Ni/Ai /1/m/ The values of N and ď. are obtained from the following relations: SX X N si = N i /A i /1/m/

5i » /m/ kde N· je počet kavit, 1 2 A^ vyšetřovaná plocha v m5i » /m/ where N· is the number of cavities, 1 2 A^ the examined area in m

I/£ celková délka středních průměrů kavit v m metalografického výbrusu sledované hladiny i .I/£ is the total length of the mean diameters of cavities in m of the metallographic section of the monitored surface i.

Celkové poškození má svou hranici, která sé navenek projeví prasknutím trubky. Lom nastane v okamžiku, kdy jsou poškození jednotlivých hladin zhruba na stejné úrovni a dosáhnou mezní hodnoty. Znalost tohoto limitního poškození je nezbytná při stanovení jak zbytkové, tak celkové životnosti materiálu. V citované studii bylo experimentálně prokázáno, že hodnota mezního poškození může být popsána geometrickým kriteriem, které není příliš závislé na působících vnějších podmínkách a významně neaévisí na typu a strukturním stavu materiálu. Mezní poškození je možno uvažovat jako stav, který bezprostředně předchází nestabilnímu (katastrofickému) vzrastu poškození. Tohoto mezního poškození se za podmínek vysokoteplotního creepu dosahuje v čase, který odpovídá asi 90% celkové životnosti materiálu. Při neměnných vnějších podmínkách lze do této doby uvažovat konstantní nárůst poškození.The total damage has its limit, which is externally manifested by the rupture of the pipe. The fracture occurs when the damage of the individual levels is approximately at the same level and reaches a limit value. Knowledge of this limit damage is necessary for determining both the residual and total service life of the material. In the cited study, it was experimentally proven that the value of the limit damage can be described by a geometric criterion that is not very dependent on the external conditions and does not significantly depend on the type and structural state of the material. Limit damage can be considered as a state that immediately precedes the unstable (catastrophic) increase in damage. This limit damage is reached under high-temperature creep conditions in a time that corresponds to about 90% of the total service life of the material. With constant external conditions, a constant increase in damage can be considered until this time.

Hodnotu mezního poškození Vmez je možno stanovit, jak již bylo uvedeno, kupříkladu rozborem creepového vzorku, u něhož došlo k lomu za podmínek blížících se podmínkám provozním, přičemž se stanoví podíl mezikrystalových dutin v činné části vzorku, mimo oblast magistrální trhliny. Pro odstředivě litý materiál procesních reformingových trubek je Vmez »0,01.The value of the limit damage V limit can be determined, as already mentioned, for example by analyzing a creep sample that has fractured under conditions close to operating conditions, while determining the proportion of intercrystalline voids in the active part of the sample, outside the area of the main crack. For centrifugally cast material of process reforming tubes, V limit is »0.01.

- 7 253 371- 7,253,371

Dále byla předběžně stanovena závislost mezi objemovým podílem kavit povrchové hladiny % a sumárním objemovým podílem kavit celé stěny trubky Vko· Aproximací výsledků metalografických rozborů stupně poškození řady vzorků (viz připojená Tabulka hodnot měření), odebraných z části reformingových trubek o 0 132x16, zhoto vených z mat· 4OCr25Ni2O, metodou nejmenších čtverců byl získán vztah i . _ v 3 kc ( a-.Furthermore, the dependence between the volume fraction of surface level cavities % and the total volume fraction of cavities of the entire tube wall V ko was preliminarily determined. By approximating the results of metallographic analyses of the degree of damage of a number of samples (see the attached Table of measurement values), taken from a part of reforming tubes of 0 132x16, made of 4OCr25Ni2O material, the relationship i . _ v 3 kc ( a-.

1/2 'kp kp * akp kde a1 « 7,0816419 a2 ~ - 7,6284424 .102 a3 = 3,1045440 · 104 1/2 'kp kp * akp where a 1 « 7.0816419 a 2 ~ - 7.6284424 .10 2 and 3 = 3.1045440 · 10 4

Kritická oblast trubky byla zjištěna z rozboru řady havarií. Ke creepovému lomu docházelo vždy pravidelně v oblasti kolmé na rovinu radiační sekce reformingové pece a to v© vzdáleností cca 200 mm od sváru mezi třetí a čtvrtou částí -(počítáno od příruby) reformingové trubky. Trhlina byla vždy orientována osově.The critical area of the tube was determined from the analysis of a number of accidents. Creep fracture always occurred regularly in the area perpendicular to the plane of the radiation section of the reformer furnace, at a distance of approximately 200 mm from the weld between the third and fourth parts (counted from the flange) of the reformer tube. The crack was always oriented axially.

Na základě výše uvedených závěrů a rozboru konkrétního případu možné aplikace byl pak stanoven obecný postup zkoušení, který může být použit při zjišťování zbytkové životnosti všech dílců a součástí, jež dlouhodobě pracují v oblasti vysokoteplotního creepu a u nichž je možno stanovit funkční závislost mezi poškozením povrchové hladiny a celkovým poškozením dílce v kritickém místě·Based on the above conclusions and the analysis of a specific case of possible application, a general testing procedure was then determined, which can be used to determine the residual life of all parts and components that operate in the high-temperature creep area for a long time and for which it is possible to determine the functional dependence between surface damage and overall damage to the part at a critical point.

Výbrus povrchu dílce či součásti je možno provést v praxi běžně zvládnutými metalografickými metodami, po předchozím odstranění provozem znehodnocené vrstvy·Opakovaný výbrus je možno provést přímo v místě prvního výbrusu anebo - z důvodů bezpečnosti- v místě bezprostředně vedle něho· Metalografické vyhodnocení stupně poškozen přímo na vyšetřovaném místě anebo pomocí otisku či fotografie plochy výbrusu, které je možno nadto i archivovat .Vyhodnocení stupně poškození je možno popřípadě výrazně zproduktivnit zavedením automatické obrazové analýzy·The surface of a part or component can be ground using commonly used metallographic methods, after previously removing the layer damaged by operation. Repeated grinding can be carried out directly at the location of the first grinding or - for safety reasons - at a location immediately next to it. Metallographic evaluation of the degree of damage directly at the examined location or using an imprint or photograph of the grinding surface, which can also be archived. The evaluation of the degree of damage can be significantly increased by introducing automatic image analysis.

Doba určenái k provedení prvního metalografického výbrusu u vyšetřovaného souboru dílců a následné vyhodnocení stupně poškozeníTime allocated for performing the first metallographic section on the examined set of parts and subsequent evaluation of the degree of damage

- 8 253 371 povrchové hladiny dílců se stejně jako interval mezi následujícími, opakovanými metalografickými vyšetřeními volí v závislosti na provozních podmínkách, zejména také s ohledem na plánované odstávky technologického zařízení· Pro stanovení termínu opakovaných měření je rozhodující kromě toho i stupeň poškození sledovaného souboru dílců, zjištěný při předchozím vyšetření· Pro konkrétní případ trubek reformingové pece se z důvodů zajištění potřebné provozní spolehlivosti zařízení interval mezi jednotlivými měřeními volí v rozmezí 1/2 až 1 1/2 roku·- 8,253,371 surface levels of parts, as well as the interval between subsequent, repeated metallographic examinations, are selected depending on the operating conditions, especially with regard to planned shutdowns of the technological equipment. In addition, the degree of damage to the monitored set of parts, detected during the previous examination, is decisive for determining the date of repeated measurements. For the specific case of reforming furnace tubes, the interval between individual measurements is selected in the range of 1/2 to 1 1/2 years in order to ensure the necessary operational reliability of the equipment.

Nový postup zjišťování zbytkové životnosti kovových materiálů umožní dokonalé, celkové vyčerpání žárupevných vlastností materiálu· Tím se docílí nejen úspory vysocelegovaného materiálu, ale i úspory energie potřebné k výrobě nového dílce, přičemž zanedbatel ná není ani úspora nákladů na dopravu a montáž tohoto dílce· Aplikace navrženého postupu přinese kromě toho bezesporu i výrazné zvýšení provozní jistoty zařízení·The new procedure for determining the residual service life of metal materials will enable perfect, total exhaustion of the refractory properties of the material. This will not only save high-alloy material, but also save energy needed to produce a new part, while the cost savings for transportation and assembly of this part are also not negligible. The application of the proposed procedure will undoubtedly also bring a significant increase in the operational reliability of the equipment.

Kromě reakčních trubek pecí pro parní reforming je možno postu pu podle vynálezu použít i pro stanovení zbytkové životnosti tzv· pig-tailů, tj· trubic, kterými je výstup reformingových trubek napojen na horký kolektor, anebo u těchto kolektorů samotných, popřípadě u trubek, trubkových hadů či haedrů ohřevných trubkových pecí· Obecně pak u všech kovových dílců, které musí dlouhodobě vydržet vysokoteplotní namáhání·In addition to reaction tubes of steam reforming furnaces, the method according to the invention can also be used to determine the residual life of the so-called pig-tails, i.e. tubes through which the outlet of the reforming tubes is connected to the hot collector, or for these collectors themselves, or for tubes, tube coils or heads of heating tube furnaces. In general, for all metal parts that must withstand high-temperature stress for a long time.

.. q ... q .

Tabulka hodnot měřeníMeasurement value table

253 371253,371

Vkp·10'3 In kp· 10 ' 3 Tke·10'3 T ke· 10 ' 3 Č.měř· Number of measures vkp·10 3 in k p · 10 3 Vkc”10 In CZK 10 0,225 0.225 63,319 63,319 31 31 0,419 0.419 37,363 37,363 1,981 1,981 109,731 109,731 33 33 0,656 0.656 46,863 46,863 0,069 0.069 5,419 5,419 33 33 0,656 0.656 67,819 67,819 0,044 0.044 14,481 14,481 34 34 4,156 4,156 137,600 137,600 0,019 0.019 6,900 6,900 35 35 0,913 0.913 85,981 85,981 0,013 0.013 6,381 6,381 36 36 0,406 0.406 22,338 22,338 0,500 0.500 81,419 81,419 37 37 0,763 0.763 38,563 38,563 0,419 0.419 66,713· 66,713· 38 38 3,619 3,619 124,919 124,919 0,156 0.156 28,181 28,181 39 39 1,213 1,213 83,300 83,300 1,994 1,994 94,619 94,619 40 40 1,044 1,044 80,838 80,838 0,956 0.956 73,538 73,538 41 41 0,538 0.538 27,881 27,881 0,419 0.419 45,338 45,338 42 42 0,156 0.156 11,519 11,519 1,719 1,719 113,363 113,363 43 43 0,281 0.281 12,681 12,681 0,406 0.406 24,981 24,981 44 44 0,000 0.000 0,000 0.000 0,131 0.131 54,719 54,719 45 45 10,000 10,000 160,000 160,000 0,750 0.750 71,781 71,781 0,225 0.225 36,919 36,919 0,256 0.256 59,038 59,038 1,713 1,713 114,881 114,881 0,275 0.275 13,663 13,663 0,175 0.175 9,719 9,719 0,625 0.625 59,981 59,981 0,894 0.894 85,081 85,081 0,625 0.625 29,663 29,663 0,731 0.731 43,819 43,819 0,388 0.388 36,481 36,481 0,819 0.819 110,381 110,381 0,281 0.281 25,463 25,463 0,994 0.994 73,963 73,963 0,638 0.638 80,363 80,363

, 10 -, 10 -

Claims (1)

Způsob nedestruktivního zjišťování zbytkové životnosti kovových materiálů u dílců dlouhodobě namáhaných vysokoteplotním creepfem, kupříkladu reakčních trubek reformingových pecí, založený na použití mikrostrukturní analýzy, vyznačený tím, žeA method of non-destructive determination of the residual life of metallic materials in parts subjected to long-term high-temperature creepf, such as reforming furnace reaction tubes, based on the use of microstructural analysis, characterized in that: a) u vyšetřovaného dílce, popřípadě souboru dílců se zjistí jejich kritické místo,a) a critical point is found in the investigated member or set of components, b) určí se mezní hodnota poškození použitého kovového materiálu a(b) the damage limit value of the metallic material used is determined; and c) stanoví se závislost poškození povrchové hladiny na jejich celkovém poškození, načež se(c) the dependence of surface level damage on their total damage is determined, whereupon d) po předem stanovené době provozu u jednotlivých vyšetřovaných dílců provede metalografický výbrus dílce v kritickém místě a. (d) after a predetermined period of operation for each component examined, metallographically cut the component at a critical point; and e) metalograficky se vyhodnotí stupeň poškození povrchové hladiny dílců, přičemž se(e) the degree of damage to the surface level of the components is evaluated by metallography, whereby: f) ze stupně zjištěného poškození povrchové hladiny dílců podle vztahu z bodu c) vypočte celkové poškození dílce, načež se(f) from the degree of damage to the surface level of the components as determined in relation to (c), calculate the total damage to the component, whereupon g) postup podle bodů d) až f) u každého ze souboru vyšetřovaných dílců nejméně jednou opakuje, přičemž ee metalografický výbrus provede opět v kritickém místě dílců, a(g) repeats the procedure under (d) to (f) for each of the components examined at least once, re-performing the metallographic cut at the critical point of the components; and h) ze srovnání časově závislého nárůstů poškození dílců a předem určeného mezního poškození užitého materiálu se odvodí zbytková životnost materiálu dílců.(h) the residual life of the component material shall be derived from a comparison of time-dependent increases in component damage and predetermined marginal damage to the material used.
CS85834A 1985-02-07 1985-02-07 Method of non-destructive determination of residual life of metallic materials CS253371B1 (en)