CS254914B1 - The way to reduce the corrosive effect of organic acids - Google Patents

The way to reduce the corrosive effect of organic acids Download PDF

Info

Publication number
CS254914B1
CS254914B1 CS859117A CS911785A CS254914B1 CS 254914 B1 CS254914 B1 CS 254914B1 CS 859117 A CS859117 A CS 859117A CS 911785 A CS911785 A CS 911785A CS 254914 B1 CS254914 B1 CS 254914B1
Authority
CS
Czechoslovakia
Prior art keywords
acids
acid
corrosion
weight
stainless steel
Prior art date
Application number
CS859117A
Other languages
Czech (cs)
Slovak (sk)
Other versions
CS911785A1 (en
Inventor
Ladislav Komora
Vendelin Macho
Eva Komorova
Original Assignee
Ladislav Komora
Vendelin Macho
Eva Komorova
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Ladislav Komora, Vendelin Macho, Eva Komorova filed Critical Ladislav Komora
Priority to CS859117A priority Critical patent/CS254914B1/en
Publication of CS911785A1 publication Critical patent/CS911785A1/en
Publication of CS254914B1 publication Critical patent/CS254914B1/en

Abstract

Sposob rieši zníženie korózie zariadenia „nerezu“. Rieši zníženie korozívnych účinkov organických kyselin aj za přítomnosti anorganických kyselin a vody na nehrdžavejúcej ocele, kde prídavkom je aspoň jedna zlúčenina prvku zo skupiny prvkov med', že'ezo, molybdén, nikel, antimon, cín, arzén v množstve 0,001 % hmot. až 1 % hmot., počítané na kvapalnú fázu prostredia, pričom zlúčeniny prvkov sú oxidy, hydroxidy alebo soli kyselin slabších alebo rovnako silných ako kyseliny prostredia, kovový cín a zo solí železa len soli dvojmocného železa. Riešenie možno využit pri přípravě, izolácii, spracovaní organických kyselin, kde znižuje koróziu zariadenia tri- až stokrát. Všade tam, kde sa používá nerezové zariadenia a práce za přítomnosti organických kyselin.The method solves the problem of reducing corrosion of "stainless steel" equipment. It solves the problem of reducing the corrosive effects of organic acids even in the presence of inorganic acids and water on stainless steel, where the additive is at least one compound of an element from the group of elements copper, iron, molybdenum, nickel, antimony, tin, arsenic in an amount of 0.001% by weight to 1% by weight, calculated on the liquid phase of the environment, where the compounds of the elements are oxides, hydroxides or salts of acids weaker or equally strong than the acids of the environment, metallic tin and from iron salts only salts of divalent iron. The solution can be used in the preparation, isolation, processing of organic acids, where it reduces corrosion of equipment by three to a hundred times. Wherever stainless steel equipment is used and work is carried out in the presence of organic acids.

Description

Vynález sa týká zníženia korozívnych účinkov organických kyselin aj za přítomnosti anorganických kyselin a vody na nehrdzavejúce ocele.The invention relates to reducing the corrosive effects of organic acids even in the presence of inorganic acids and water on stainless steels.

Je známe, že pri výrobě, resp. spracovaní organických kyselin, najma pri vyšších teplotách, je potřebné používat legované, či iné materiály z nehrdzavejúcej ocele, obvykle s velkým obsahom chrómu, resp. chrómu a molybdenu [Donndorf R. a kol. (překlad z německého originálu): Volba materiálu a protikorozní ochrana v chemickém průmyslu, SNTL Praha 1980]. Najlepšie o dolávajú korózii kyselinou octovou niklové zliatiny (NiFe220r22Mo) a titán, a to aj za přítomnosti oxidačných alebo redukčných příměsí. Titán a tantal odolávajú najlepšie kyselině octovej všetkých koncentrácií až do teploty varu. Rozpuštěný kyslík a iné oxidačné látky majú pasivačný účinok na korozivzdornú ocel'. Tak rýchlosť korózie v technickej 1'adovej kyselině octovej neprevzdušnenej je 0,081 mm . rok-1, zatial' čo prevzdušnenej 0,00 mm . rok“1 materiálu X8CrNiMoTil8 11 (ČSN 17 348). Odolnost voči parám sa za přítomnosti kyslíka zvyšuje 2,6-krát. Podobné působia aj iné oxidujúce látky, ako manganistan sodný, peroxid vodíka, dvojchroman sodný a ortuťnaté soli.It is known that in the production or processing of organic acids, especially at higher temperatures, it is necessary to use alloyed or other stainless steel materials, usually with a high content of chromium or chromium and molybdenum [Donndorf R. et al. (translation from the German original): Material selection and corrosion protection in the chemical industry, SNTL Prague 1980]. Nickel alloys (NiFe220r22Mo) and titanium are best resistant to corrosion by acetic acid, even in the presence of oxidizing or reducing impurities. Titanium and tantalum are best resistant to acetic acid of all concentrations up to the boiling point. Dissolved oxygen and other oxidizing substances have a passivating effect on stainless steel. Thus, the corrosion rate in non-aerated technical grade acetic acid is 0.081 mm . year -1 , while in aerated 0.00 mm . year” 1 of the material X8CrNiMoTil8 11 (ČSN 17 348). Resistance to vapors increases 2.6 times in the presence of oxygen. Other oxidizing substances, such as sodium permanganate, hydrogen peroxide, sodium dichromate and mercury salts, have a similar effect.

Korózia materiálov z nehrdzavejúcej ocele organickými kyselinami je nezriedka vyššia za přítomnosti vody ako v koncentrovaných kyselinách [Tabulky korozní odolnosti ocelí Poldi anticorr. Vydali Spojené ocelárny, n. p., Kladno (1970)]. Tak, zatial' čo pre koncentrovaná kyselinu octovú za varu materiály Poldi AK 1 (ČSN 17 021), AK 2S (ČSN 17 022), AK 3R (ČSN 17 023), AK 4R (ČSN 17 024) niekedy vyhovujú, pre kyselinu octovú o konc. 50 % hmot. nevyhovujú. Podobné, odolnosti AK lNi, AK lBe [ČSN 17 041, AK V (ČSN 17 460), AK VN (ČSN 17 241), AK V8 (ČSN 17 240), AK VS 10 (ČSN 17 248) voči koncentrovaným roztokom je dobrá, za přítomnosti vody vyhovuje len zriedkavo. Kyselině mliečnej za varu odolávajú len výrobky Poldi AK VEextra (ČSN 17 346), AK VUltra (ČSN 17 352) a AK VSuper (ČSN 17 356), zatial' čo iné vyhovujú len niekedy. Pre kyselinu mravčiu za varu vyhovujú už len materiály AK VUltra (ČSN 17 350) a kyselině šťavelovej za varu len Poldi Akor (ČSN 17 252). Vodnému roztoku kyseliny sírovej o konc. 5 °/o hmot. za varu vyhovuje len materiál Poldi Akor (ČSN 17 252), zatial' čo ostatně materiály z nehrdzavejúcej ocele buď nevyhovujú vóbec, alebo len čiastočne. Kyselině fosforečnej o koncentrácií 50 % hmot. za varu vyhovujú len materiály AK VExtra (CSN 17 346), AK VUltra (ČSN 17 352), AK VSuper (ČSN 17 356). Kyselině dusičnej o konc. 65 % hmot. za varu tiež vyhovujú len niektoré druhy materiálov. Ani v jednom případe nie je odolnost materiálov velmi dobrá (klasifikačně číslo 0).Corrosion of stainless steel materials by organic acids is often higher in the presence of water than in concentrated acids [Tables of corrosion resistance of Poldi anticorr steels. Published by Spojené ocelárny, n. p., Kladno (1970)]. Thus, while for concentrated acetic acid at boiling point the materials Poldi AK 1 (ČSN 17 021), AK 2S (ČSN 17 022), AK 3R (ČSN 17 023), AK 4R (ČSN 17 024) are sometimes suitable, for acetic acid with a concentration of 50% by weight they are not suitable. Similarly, the resistance of AK lNi, AK lBe [ČSN 17 041, AK V (ČSN 17 460), AK VN (ČSN 17 241), AK V8 (ČSN 17 240), AK VS 10 (ČSN 17 248) to concentrated solutions is good, in the presence of water it is only rarely suitable. Only Poldi AK VEextra (ČSN 17 346), AK VUltra (ČSN 17 352) and AK VSuper (ČSN 17 356) products withstand boiling lactic acid, while others are only sometimes suitable. For boiling formic acid, only AK VUltra (ČSN 17 350) materials are suitable, and for boiling oxalic acid, only Poldi Akor (ČSN 17 252). For an aqueous solution of sulfuric acid with a conc. 5 %/o mass. only Poldi Akor material (ČSN 17 252) is suitable for boiling, while other stainless steel materials either do not comply at all or only partially. Phosphoric acid with a concentration of 50% by weight is only suitable for boiling for AK VExtra (CSN 17 346), AK VUltra (ČSN 17 352), AK VSuper (ČSN 17 356). Nitric acid with a concentration of 65% by weight is also only suitable for boiling for some types of materials. In neither case is the resistance of the materials very good (classification number 0).

Ako inhibitory korózie kyslým prostředím sú známe chrómany, fosforečnany, dibenzylsulfoxid, hexametyléntetramín, deriváty močoviny, pyridin, chinolín, aminy [Donndorf a kol.: Volba materiálu a protikorozní ochrana v chemickém průmyslu, SNTL Praha, (1980)] a oxidačně látky. Ako sme sa však přesvědčili niektoré z nich, napr. dusičnany a peroxidy po počiatočnej inhibícii, po 20 h nielenže už neposobia inhibične, ale naopak, zvyšujú koróziu v porovnaní s kontrolnými vzorkami materiálov bez přítomnosti oxidačných látok.As inhibitors of corrosion in acidic environments, chromates, phosphates, dibenzyl sulfoxide, hexamethylenetetramine, urea derivatives, pyridine, quinoline, amines [Donndorf et al.: Material selection and corrosion protection in the chemical industry, SNTL Prague, (1980)] and oxidizing agents are known. However, as we have seen, some of them, e.g. nitrates and peroxides, after initial inhibition, after 20 h not only no longer act as inhibitors, but on the contrary, increase corrosion compared to control samples of materials without the presence of oxidizing agents.

Inhibitory voči posobeniu organických kyselin nie sú vo všeobecnosti známe. Pre kyselinu šťavelovú je chráněné použitie štavelanu železitého ako zlúčeniny trojmocného železa (US patent 2 793 190). Jeho použitie móže mať inhibičný účinok voči korózii nerezových materiálov, ale z hladiska výroby resp. dostupnosti šťavelanu železitého je jeho použitie velmi obmedzené.Inhibitors against the action of organic acids are not generally known. For oxalic acid, the use of ferric oxalate as a trivalent iron compound is protected (US patent 2,793,190). Its use may have an inhibitory effect against the corrosion of stainless steel materials, but from the point of view of the production or availability of ferric oxalate, its use is very limited.

Nakoíko korózia sposobuje značné technické problémy a národohospodářské škody a na výrobu vačšiny zariadení chemických výrobní sú vhodné len vysokolegované materiály z nehrdzavejúcej ocele a navýše aj u týchto dochádza poměrně k značnej korózii a tým zníženiu životnosti, pokusili sme sa nájsť také riešenie, ktorým sa výrazné zvýšila odolnost nehrdzavejúcich ocelí, hlavně voči agresívnym chemikáliám.Since corrosion causes significant technical problems and economic damage, and only high-alloy stainless steel materials are suitable for the production of most chemical production equipment, and even these also experience relatively significant corrosion and thus a reduction in service life, we tried to find a solution that would significantly increase the resistance of stainless steels, especially against aggressive chemicals.

Uvedené problémy rieši spósob podfa tolito vynálezu.The above problems are solved by the method according to the invention.

Podfa tohto vynálezu sa spósob zníženia korozívneho účinku organických kyselin i za přítomnosti anorganických kyselin a vo dy na nehrdzavejúcej,. ocele, uskutočňuje tak, že sa do prostredia obsahujúceho kyselinu alebo zmes kyselin jednorázové alebo po častiach přidává inhibitor korózie v množstve 0,001 až 1 % hmot., počítané na kvapalnú fázu prostredia, pričom inhibítorom je aspoň jedna zlúčenina prvku zo skupiny prvkov meď, železo, molybden, nikel, antimon, cín, arzén, pričom zlúčeniny prvkov sú oxidy, hydroxidy alebo soli kyselin slabších alebo rovnako silných ako kyseliny prostredia, kovový cín a zo soli železa len soli dvojmocného železa.According to the present invention, the method of reducing the corrosive effect of organic acids even in the presence of inorganic acids and water on stainless steel is carried out by adding a corrosion inhibitor to the medium containing an acid or a mixture of acids, either once or in parts, in an amount of 0.001 to 1% by weight, calculated on the liquid phase of the medium, wherein the inhibitor is at least one compound of an element from the group of elements copper, iron, molybdenum, nickel, antimony, tin, arsenic, wherein the compounds of the elements are oxides, hydroxides or salts of acids weaker or equally strong than the acids of the medium, metallic tin, and from iron salts only salts of divalent iron.

Výhodou postupu podl'a tohto vynálezu je technicky nenáročné a přitom výrazné zníženie korozívnych účinkov organických kyselin, ale aj ich zmesi s anorganickými kyselinami na nehrdzavejúce ocele. Viackrát sa predlži životnost zariadení a zvýši sa prevádzková spofahlivosť a bezpečnost' výrobných procesov.The advantage of the method according to the present invention is that it is technically undemanding and at the same time significantly reduces the corrosive effects of organic acids, as well as their mixtures with inorganic acids, on stainless steels. The service life of the equipment is extended several times and the operational reliability and safety of the production processes are increased.

Spósob podfa tohto vynálezu je velmi jednoduchý a technicky nenáročný, nakoíko prídavok alebo přídavky prvkov alebo zlúčenín prvkov premenlivého mocenstva i v malom množstve znižuje koróziu nehrdzavejúcich ocelí desať- i viackrát. Přitom množstvo inhibítora v korodujúcom prostředí je vhodné použiť v koncentrácii 0,001 až 1 % hmot., najlepšie však 0,01 až 0,2 % hmot., počítané na zmes obsahujúcu kyselinu. Postup je zvlášť vhodný pri výrobě, rektifikácii, ako aj rafinácii kyselin a ich anhydridov, ako aj pri reakciách za přítomnosti re·· agujúcich, či generovaných kyselin.The method according to the present invention is very simple and technically undemanding, since the addition or additions of elements or compounds of elements of variable valency even in small amounts reduces the corrosion of stainless steels by ten or more times. The amount of inhibitor in the corrosive environment is preferably used in a concentration of 0.001 to 1% by weight, but preferably 0.01 to 0.2% by weight, calculated on the mixture containing the acid. The method is particularly suitable for the production, rectification, and refining of acids and their anhydrides, as well as for reactions in the presence of reacting or generated acids.

Podťa tohto vynálezu ide o zníženie či potlačenie korozívneho účinku na nehrdzavejúcu ocel’, organickej a anorganickej kyše liny, organických a anorganických kyselin, pričom pod pojmoin kyselina alebo kyseliny sa rozume jú aj anhydridy kyseliny, ako aj kyseliny vytvárajúce „in šitu“, napr. chemickými reakcianii. Korodujňce prostredie móže obsahovat z kvantitativného hladiska v podstatě len nekorodujúce 'útky a zlúče niny, pričom koróziu sposobuje len příměs aspoň jednej kyseliny, ktorá dokonca meze vzniknúť napr. hydrolýzou esterov so vzdušnou vlhkostmi, či oxidáciou aldehydov vzduchom ap.The present invention concerns the reduction or suppression of the corrosive effect on stainless steel of organic and inorganic acids, organic and inorganic acids, whereby the term acid or acids also includes acid anhydrides, as well as acids formed "in situ", e.g. by chemical reactions. A corrosive environment may contain from a quantitative point of view essentially only non-corrosive substances and compounds, whereby corrosion is caused only by the admixture of at least one acid, which may even arise e.g. by hydrolysis of esters with atmospheric moisture, or oxidation of aldehydes by air, etc.

Inhibitor korózie sa do prostredia obsahujúceho aspoň jednu kyselinu alebo zmes kyselin přidává jednorázové alebo po častiach, teda diskontinuálne, polokontinuálne alebo kontinuálně. Přitom pod jednorázovým přidáním rozumieme tiež predsadenio do prostredia či aparátu, do ktorého sa dodatečné privedie médium,· obsahujúce a/alebo vytvárajúce kyselinu alebo kyseliny. V polokontinuálnych a kontinua nych procesoch je vhodné inhibitor korózie přidával samotné alebo spolu s východiskovými surovinami. Vhodnejšie, najmá ak ide o zlúčeniny, je ich dávkovanie spolu s východiskovou surovinou, v ktorej sa lepšie rozpúšťa.The corrosion inhibitor is added to the medium containing at least one acid or a mixture of acids in one go or in portions, i.e. discontinuously, semi-continuously or continuously. In this case, by one go we also mean pre-addition to the medium or apparatus into which the medium containing and/or forming the acid or acids is additionally fed. In semi-continuous and continuous processes, it is appropriate to add the corrosion inhibitor alone or together with the starting materials. It is more suitable, at least in the case of compounds, to dose them together with the starting material in which it dissolves better.

Najvhodnejšie je použit jeden alebo viac prvkov vo formě ich zlúčenín, ako oxidov, hydroxidov, uhlíčitanov alebo solí, připadne koordinačných zlúčenín. Pri volbě solí je vhodné volil ich kvalitu v závislosti od druhu kyseliny, alebo zmesi kyselin, voči korozívnemu účinku, ktorých je zapotreby zariadenie chránil. Přitom zásadné neodporúčame, a to je podstatou vynáezu, aplikoval soli silnějších kyselin, napr. anorganických, ak tieto nie sú přítomné v reakčnom prostředí, voči ktorému je třeba zariadenie chránit, Z uvedených dóvodov sa vyhýbáme použitiu chloridov prvkov s proměnlivým mocenstvom, připadne síranov, ak sa zabraňuje korózii len napr. samotnou organickou kyselinou alebo zmesou len organických kyselin. Přitom třeba však zohladniť i rozpustnost príslušnej soli vo vodě alebo organickej kyselině, ktorej účinok korózie potláčame. Nerešpektovanie tohto postupu βIt is most appropriate to use one or more elements in the form of their compounds, such as oxides, hydroxides, carbonates or salts, or coordination compounds. When choosing salts, it is appropriate to choose their quality depending on the type of acid, or mixture of acids, against the corrosive effect of which the device needs to be protected. In this case, we fundamentally do not recommend, and this is the essence of the invention, applying salts of stronger acids, e.g. inorganic, if these are not present in the reaction medium against which the device needs to be protected. For the reasons stated, we avoid using chlorides of elements with variable valency, or sulfates, if corrosion is prevented only, e.g. by the organic acid itself or by a mixture of only organic acids. However, the solubility of the respective salt in water or the organic acid, the corrosion effect of which is suppressed, must also be taken into account. Failure to comply with this procedure β

by mohlo zavinil, že předpokládaný inhibitor korózie v niektorých prípadoch by bol neúčinný alebo dokonca by mohol ešte koróziu zrýclťiť.could cause the intended corrosion inhibitor to be ineffective in some cases or could even accelerate corrosion.

Spósob podlá tohto vynálezu sa dá používat v diskontinuálnom, polokontinuálnom, kontlnuálnom zariadení. Vhodný je tiež aj na ochranu zariadení hlavně z nehrdzavejúcej ocele pri dlhodobom pósobení korodujúcich médií, ako napr. pri skladovaní kyselin na ochranu zásobníkov, absorpčných kolon kyslých plynov ap. Přitom, ak sa jedná napr. o ochranu varáka destilačnej kolóny, stačí jednorázový prídavok inhibítora do varáka kolóny; inhibitor je stály, a teda má ochranný účinok až po výměnu násady varáka.The method according to the present invention can be used in discontinuous, semi-continuous, continuous equipment. It is also suitable for the protection of equipment mainly made of stainless steel during long-term exposure to corrosive media, such as when storing acids to protect tanks, absorption columns of acid gases, etc. In this case, if it is e.g. the protection of the distillation column reboiler, a single addition of the inhibitor to the column reboiler is sufficient; the inhibitor is permanent and therefore has a protective effect until the reboiler head is replaced.

Uskutočnenie postupu podlá tohto vynálezu, ako aj ďalšie podrobnosti i výhody, objasňujú příklady, ktoré však nevyčerpávajú všetky možné kombinácie.The implementation of the process according to the invention, as well as further details and advantages, are illustrated by the examples, which, however, do not exhaust all possible combinations.

Příklad 1Example 1

V banke o objeme 200 cm3 opatrenej spatným chladičom a teplomerom sa skúšajň materiály z nehrdzavejúcej ocele podlá ČSN 17 246 a ČSN 17 347 na koróziu účinkom kyseliny octovej s prídavkami roznych anorganických kyselin.In a flask with a volume of 200 cm 3 equipped with a negative condenser and a thermometer, stainless steel materials are tested according to ČSN 17 246 and ČSN 17 347 for corrosion by the effect of acetic acid with additions of various inorganic acids.

Podlá ČSN 17 246 materiál z nehrdzavejúcej ocele obsahuje menej ako 0,12 % hmot. uhlíka, menej ako 2,0 % hmot. manganu, menej ako 1,0 % hmot. kremíka, 17,0 až 20,0 °/o hmot. chrómu, 8,0 až 11,0 % hmot. niklu, viac ako 0,36 % hmot. titánu. Materiál „nerez“ ČSN 17 347 obsahuje menej ako 0,12 % hmot. uhlíka, menej ako 2,0 % hmot. manganu, menej ako 1,5 % hmot. kremíka, 16,0 až 19,0 % hmot. chrómu, 9 až 12 % hmot. niklu, 1,5 až 2,5 % hmot. molybdénu, viac ako 0,6 % hmot. titánu.According to ČSN 17 246, stainless steel material contains less than 0.12% by weight of carbon, less than 2.0% by weight of manganese, less than 1.0% by weight of silicon, 17.0 to 20.0% by weight of chromium, 8.0 to 11.0% by weight of nickel, more than 0.36% by weight of titanium. The material "stainless steel" ČSN 17 347 contains less than 0.12% by weight of carbon, less than 2.0% by weight of manganese, less than 1.5% by weight of silicon, 16.0 to 19.0% by weight of chromium, 9 to 12% by weight of nickel, 1.5 to 2.5% by weight of molybdenum, more than 0.6% by weight of titanium.

Skúšobné teliesko po zvážení (rozměry 40 X 10 X 1 mm, povrch 900 mm2) sa ponoří do 50 g roztoku kyseliny v banke po dobu 8 h. Teplota vyhrievacieho kúpela je 110 °C. Po 8 h sa obsah banky ochladí a teliesko sa odváži. Hmotnostný úbytok sa přepočítá na g . m-2 . h-1. Skúšky prebiehajú podlá množstva úbytku materiálu z nehrdzavejúcej ocele od 16 do 100 h. Dosiahnuté výsledky vplyvu přísad anorganických kyselín v kyselině octovej o konc. 50 % hmot., druhu a množstva inhibítorov na úbytok „nerezu“ ČSN 17 246 pri teplote 100 +0,2 °C sú prehladne uvedené v tabulke 1.The test specimen after weighing (dimensions 40 X 10 X 1 mm, surface 900 mm 2 ) is immersed in 50 g of acid solution in a flask for 8 h. The temperature of the heating bath is 110 °C. After 8 h, the contents of the flask are cooled and the specimen is weighed. The weight loss is converted to g . m -2 . h -1 . The tests are carried out according to the amount of loss of stainless steel material from 16 to 100 h. The results achieved of the influence of inorganic acid additives in acetic acid with a concentration of 50% by weight, the type and amount of inhibitors on the loss of "rust" ČSN 17 246 at a temperature of 100 +0.2 °C are clearly shown in Table 1.

Tabu tkalTaboo weaved

Druh anorganickej kyseliny Type of inorganic acid Koncentrácia anorganickej kyseliny [θ/o hmot.] Inorganic acid concentration [θ/wt.] 1 1 2 2 chlorovodíková hydrochloric acid 5,0 5.0 chlorovodíková hydrochloric acid 5,0 5.0 chlorovodíková hydrochloric acid 5,0 5.0 fosforečná phosphoric 5,0 5.0 fosforečná phosphoric 5,0 5.0 fosforečná phosphoric 5,0 5.0 fosforečná phosphoric 5,0 5.0 dusičná nitrogen 65,0 65.0 dusičná nitrogen 65,0 65.0 dusičná nitrogen 65,0 65.0 sírová sulfurous 5,0 5.0 sírová sulfurous 5,0 5.0 sírová sulfurous 5,0 5.0 sírová sulfurous 5,0 5.0 sírová sulfurous 5,0 5.0 sírová sulfurous 5,0 5.0 sírová sulfurous 5,0 5.0 sírová sulfurous 5,0 5.0 sírová sulfurous 5,0 5.0

Z výsledkov v tabulke 1 vidno, že aj keď za přítomnosti kyseliny chlorovodíkovej οχιά měďnatý a cín znižujú koróziu „nerezu“ na polovicu, predsa je len materiál korozívne pre také prostredie nevyhovujúci (úbytok materiálu nad 10 g . rn2 . h_1J. Pri aplikácii prídavkov kyseliny fosforečnej je korozívna odolnost' velmi dobrá (do 0,1 g . . m~2 . h + . Pri skúšaní prídavkov kyseliny dusičnéj prídavok arzénu a antimónu umož ňuje preradenie materiálu z odolnosti dohřej (úbytok materiálu 0,1 až 1,0 g . nr 2 . . h~’) na velmi dobrú. Najvýraznejší je však účinok prídavkov inhibítorov korózie za použitia kyseliny sírovej, kde přídavky cínu,The results in Table 1 show that even though in the presence of hydrochloric acid, cupric and tin reduce the corrosion of "stainless steel" by half, the material is still corrosively unsuitable for such an environment (loss of material over 10 g . rn 2 . h _1 J. When applying phosphoric acid additives, the corrosion resistance is very good (up to 0.1 g . . m~ 2 . h + . When testing nitric acid additives, the addition of arsenic and antimony allows the material to be reclassified from poor resistance (loss of material 0.1 to 1.0 g . nr 2 . . h~') to very good. However, the most significant effect is the addition of corrosion inhibitors using sulfuric acid, where tin additives,

Prídavok inhibítora korózie Corrosion inhibitor additive Obytok materiálu [g ,m-2. h-1] 5 Density of material [g,m -2.h - 1 ] 5 druh 3 type 3 množstvo na kyselinu [°/o hmot.] 4 amount per acid [% by weight] 4 — — 0,00 0.00 51,9 51.9 CužO Foreign 0,20 0.20 30,5 30.5 Sn Sn 0,20 0.20 23,1 23.1 — — 0,00 0.00 0,550 0.550 CU2O CU2O 0,20 0.20 0,036 0.036 Sn Sn 0,20 0.20 0,021 0.021 Fe2O3 Fe2O3 0,20 0.20 0,028 0.028 — — 0,00 0.00 0,605 0.605 AS2Ď3 AS2Ï3 0,20 0.20 0,000 0.000 SĎ2O3 S2O3 0,20 0.20 0,000 0.000 — — 0,00 0.00 50,5 50.5 Sn Sn 0,20 0.20 0,15 0.15 AS2Ď3 AS2Ï3 0,20 0.20 0,31 0.31 Sb2Ď3 Sb2Ï3 0,20 0.20 0,18 0.18 CuSCh CuSCh 1,00 1.00 0,05 0.05 CuSOá CuSOá 0,10 0.10 0,05 0.05 CuSO4 CuSO4 0,01 0.01 0,06 0.06 Fe2Ď3 Fe2Ï3 0,05 0.05 0,06 0.06 CuSOi CuSOi 0,001 0.001 0,10 0.10 oxidu arzenitého a oxidu arsenic oxide and oxide antimonitého pre antimony for

súvajú materiál z nevyhovujúceho na dobrý a so solami médi a zlúčeninami železa na velmi dobrý.They move the material from unsatisfactory to good and, with copper salts and iron compounds, to very good.

Příklad 2Example 2

V zariadení špecifikovanom v příklade 1 sa odskúšava korózia materiálu z nehrdzavejúcich ocelí samotnými organickými kyselinami. Výsledky vplyvu organických kyselin, druhu a množstva inhibítorov na koróziu materiálov pri teplote 100 °C +0,2 ;,C sú uvedené v tabulke 2 a 3.The corrosion of stainless steel materials by organic acids alone is tested in the apparatus specified in Example 1. The results of the influence of organic acids, type and amount of inhibitors on the corrosion of materials at a temperature of 100 °C +0.2 ° C are given in Tables 2 and 3.

5 4 9145 4 914

Tabulka 2Table 2

Druh organickej kyseliny Type of organic acid Koncentrácia organickej kyseliny [ % hmot. ] Organic acid concentration [% wt. ] Prídavok inhibítora korózie Corrosion inhibitor additive Druh materiálu „nerez“ Material type: "stainless steel" Úbytok materiálu [g . m“2. h Material loss [g . m“ 2 . h druh species množstvo na kyselinu [% hmot.] amount per acid [% by weight] 1 1 2 2 3 3 4 4 5 5 6 6 octová acetic 50 50 — — 0,0 0.0 17 347 17,347 0,55 0.55 octová acetic 50 50 N1CO3 N1CO3 0,2 0.2 17 347 17,347 0,016 0.016 octová acetic 50 50 (ΝΗ4]6Μθ7θ24 (NH4]6Mθ7θ24 0,2 0.2 17 347 17,347 0,032 0.032 octová acetic 50 50 Fe2O3 Fe2O 3 0,2 0.2 17 347 17,347 0,49 0.49 octová acetic 50 50 NH4VO3 NH4VO3 0,2 0.2 17 347 17,347 0,76 0.76 octová acetic 50 50 (CH3COO)2Cu (CH3COO)2Cu 1,0 1.0 17 347 17,347 0,07 0.07 octová acetic 50 50 (CH3COOÍ2GU (CH3COOÍ2GU 0,1 0.1 17 347 17,347 0,08 0.08 octová acetic 50 50 (CH3COO)2Cu (CH3COO)2Cu 0,01 0.01 17 347 17,347 0,09 0.09 octová acetic 50 50 (CH3COO)2Fe (CH3COO)2Fe 1,0 1.0 17 347 17,347 0,09 0.09 mravčia ants 99,7 99.7 — — 0,0 0.0 17 246 17,246 0,29 0.29 mravčia ants 99,7 99.7 CU2O CU2O 0,2 0.2 17 246 17,246 0,05 0.05 mravčia ants 80 80 — — 0,0 0.0 17 246 17,246 2,38 2.38 mravčia ants 80 80 CuQ CuQ 0,2 0.2 17 246 17,246 0,05 0.05 mravčia ants 80 80 Fe2O3 Fe2O3 ​ 0,2 0.2 17 246 17,246 0,09 0.09 šťavelová sorrel 20 20 — — 0,0 0.0 17 246 17,246 0,43 0.43 šťavelová sorrel 20 20 CuO CuO 0,2 0.2 17 246 17,246 0,51 0.51 šťavelová sorrel 20 20 Fe2O3 Fe2O3 0,2 0.2 17 246 17,246 0,10 0.10 mliečna milk 100 100 — — 0,0 0.0 17 246 17,246 0,70 0.70 mliečna milk 100 100 CuO CuO 0,5 0.5 17 246 17,246 0,04 0.04 mliečna milk 100 100 Fe2O3 Fe2O3 0,5 0.5 17 246 17,246 0,24 0.24 octová acetic 100 100 —. —. 0,0 0.0 17 347 17,347 0,90 0.90 octová acetic 100 100 vzduch air — — 17 347 17,347 0,78 0.78 octová acetic 100 100 CuO CuO 0,2 0.2 17 347 17,347 0,11 0.11 octová acetic 100 100 Cu2O Cu2O 0,2 0.2 17 347 17,347 0,08 0.08 octová acetic 100 100 Fe2O3 Fe2O3 0,2 0.2 17 347 17,347 0,73 0.73 octová acetic 100 100 (CH3COO)2Fe ( CH3COO ) 2Fe 0,2 0.2 17 347 17,347 0,03 0.03 octová acetic 100 100 — — 0,0 0.0 17 246 17,246 2,24 2.24 octová acetic 100 100 vzduch air — — 17 246 17,246 2,52 2.52 octová acetic 100 100 CuO CuO 0,2 0.2 17 246 17,246 0,14 0.14

Tabulka 3Table 3

Druh Type Koncentrácia Concentration Prídavok inhibítora korózie Corrosion inhibitor additive Druh Type Úbytok Decline organickej organic organickej organic druh species množstvo quantity materiálu material materiálu material kyseliny acids kyseliny [% hmot.] acids [% wt.] na kyselinu [O/o hmot.] on acid [W/W] „nerez“ "stainless steel" [g . m~2 . tr [g . m~ 2 . tr octová acetic 100 100 CU2O CU2O 0,2 0.2 17 246 17,246 0,01 0.01 octová acetic 100 100 Fe2O3 Fe2O3 0,2 0.2 17 246 17,246 2,25 2.25 octová acetic 100 100 (CH3COO)2Fe ( CH3COO ) 2Fe 0,2 0.2 17 246 17,246 0,63 0.63 tereftalová terephthalic 50 50 — — 0,0 0.0 17 246 17,246 0,35 0.35 tereftalová terephthalic 50 50 Cu20 Cu 2 0 0,1 0.1 17 246 17,246 0,10 0.10 maleinová maleic 100 100 — — 0,0 0.0 17 246 17,246 0,92 0.92 maleinová maleic 100 100 Cu2O Cu2O 0,2 0.2 17 246 17,246 0,01 0.01 maleinová maleic 100 100 Fe2O3 Fe2O3 0,2 0.2 17 246 17,246 0,01 0.01 maleinová maleic 100 100 AS2O3 AS2O3 0,2 0.2 17 246 17,246 0,01 0.01 maleinová maleic 100 100 — — 0,0 0.0 17 347 17,347 0,31 0.31 maleinová maleic 100 100 Cu2O Cu2O 0,2 0.2 17 347 17,347 0,01 0.01 maleinová maleic 100 100 Fe2O3 Fe2O3 0,2 0.2 17 347 17,347 0,01 0.01 maleinová maleic 100 100 AS2O3 AS2O3 0,2 0.2 17 347 17,347 0,01 0.01

Skúšky s kyselinou tereftalovou sa robia v sklenenej nádobě umiestnenej v autokláve pri teplote 280 °C a s kyselinou maleinovou pri teplote 180 °C. Ako vyplývá z výsledkov tabulky 2 a 3, na zníženie korózie materiálu triedy 17 347 pri použití organických kyselin, najma za přítomnosti vodných roztokov kyseliny octovej, kyseliny mravčej, kyseliny mliečnej, oxid meďný a oxid meďnatý, resp. soli médi, znižujú rýchlosť korózie desať- až dvestokrát. V případe kyseliny tereftalovej je to 3,5-násobok. Pri použití kyseliny šťavelovej sa účinok neprejavuje, nakolko šťavelany sú vo vodě nerozpustné. V tomto případe je výhodnejšie použit zlúčeniny železa, t. j. oxidy, uhličitany, resp. soli železnaté.Tests with terephthalic acid are carried out in a glass vessel placed in an autoclave at a temperature of 280 °C and with maleic acid at a temperature of 180 °C. As follows from the results of Tables 2 and 3, to reduce the corrosion of material class 17 347 when using organic acids, especially in the presence of aqueous solutions of acetic acid, formic acid, lactic acid, copper oxide and cupric oxide, or copper salts, reduce the corrosion rate ten to two hundred times. In the case of terephthalic acid, it is 3.5 times. When using oxalic acid, the effect is not manifested, since oxalates are insoluble in water. In this case, it is more preferable to use iron compounds, i.e. oxides, carbonates, or ferrous salts.

Příklad 3Example 3

V zariadení podlá příkladu 1 sa odskúšava vplyv prídavkov inhibítorov, resp. potencionálnych inhibítorov korózie na koróziu nehrdzavejúcej ocele „nerezu“ 17 246 a 17 347 za přítomnosti vodného roztoku kyseliny šťavelovej o koncentrácii 10 % hmot. pri teplote 100 +0,2 °C. Za dobu skůšok 40 hodin sú hmotnostně straty teliesok o povrchu 900 mm2 od 0,0008 do 0,0253 g. Dosiahnuté výsledky vplyvu vodného roztoku kyseliny šťavelovej o koncentrácii 10 % hmot. a prídavkov inhibítorov v množstve 0,2 % hmot. (počítané na kyselinu šťavelovú) na koróziu nehrdzavejúcej ocele sú v tabulke 4.In the device according to example 1, the influence of the addition of inhibitors, or potential corrosion inhibitors, on the corrosion of stainless steel "stainless" 17 246 and 17 347 is tested in the presence of an aqueous solution of oxalic acid with a concentration of 10% by weight at a temperature of 100 +0.2 °C. During the test period of 40 hours, the mass losses of the bodies with a surface area of 900 mm 2 are from 0.0008 to 0.0253 g. The results obtained on the influence of an aqueous solution of oxalic acid with a concentration of 10% by weight and the addition of inhibitors in an amount of 0.2% by weight (calculated on oxalic acid) on the corrosion of stainless steel are shown in Table 4.

Druh přípravku inhibítora korózie nehrdzavejúcej oceleType of stainless steel corrosion inhibitor preparation

Tabulka 4Table 4

Druh ocele Obytok nehrdzavejúcej ocele [g . m-2. h_1]Steel type Stainless steel housing [g . m -2 . h _1 ]

bez přídavku inhibítora without added inhibitor 17 246 17,246 0,703 0.703 Sn Sn 17 246 17,246 0,236 0.236 Sb2O3 Sb2O3 17 246 17,246 0,170 0.170 AS2O3 AS2O3 17 246 17,246 0,220 0.220 NÍCO3 NOTHING3 17 246 17,246 0,260 0.260 (ΝΗ4)βΜθ7θ24 (NH4)βMθ7θ24 17 246 17,246 0,130 0.130 bez přídavku inhibítora without added inhibitor 17 347 17,347 0,290 0.290 Sn Sn 17 347 17,347 0,022 0.022 Sb2O3 Sat 2 O3 17 347 17,347 0,180 0.180 AS2O3 AS2O3 17 347 17,347 0,080 0.080 N1CO3 N1CO3 17 347 17,347 0,110 0.110 (NH4J6MO7O24 (NH4J6MO7O24 17 347 17,347 0,080 0.080

PREDMETSUBJECT

Claims (1)

PREDMETSUBJECT Spůsob zníženia korozívneho účinku organických kyselin i za přítomnosti anorganických kyselin a vody na nehrdzavejúce ocele, vyznačujúci sa tým, že sa do prostredia obsahujúceho kyselinu alebo zmes kyselin jednorázové alebo po častiach přidává inhibitor korózie v množstve 0,001 až 1 pere. hmot., počítané na kvapalnú fázu provynAlez u stredia, pričom inhitaítorom je aspoň jedna zlúčenina prvku zo skupiny prvkov med, železo, molybden, nikel, antimón, cín, arzén, pričom zlúčeniny prvkov sú oxidy, hydroxidy alebo soli kyselin slabších alebo rovnako silných ako kyse’iny prostredia, kovový cín a zo soli železa len soli dvojmocného železa.A method of reducing the corrosive effect of organic acids even in the presence of inorganic acids and water on stainless steels, characterized in that a corrosion inhibitor in an amount of 0.001 to 1 pens is added to the medium containing the acid or mixture of acids in one portion or in portions. % by weight, calculated on the liquid phase of provynAlez at the center, wherein the inhaler is at least one compound of an element from the group of elements honey, iron, molybdenum, nickel, antimony, tin, arsenic, wherein the element compounds are oxides, hydroxides or environmental acids, metallic tin and only iron (II) salts from iron salts.
CS859117A 1985-12-11 1985-12-11 The way to reduce the corrosive effect of organic acids CS254914B1 (en)