CS260744B1 - Charge for the production of refractory ceramics - Google Patents

Charge for the production of refractory ceramics Download PDF

Info

Publication number
CS260744B1
CS260744B1 CS874015A CS401587A CS260744B1 CS 260744 B1 CS260744 B1 CS 260744B1 CS 874015 A CS874015 A CS 874015A CS 401587 A CS401587 A CS 401587A CS 260744 B1 CS260744 B1 CS 260744B1
Authority
CS
Czechoslovakia
Prior art keywords
boron nitride
mixture
carbide
charge
prepared
Prior art date
Application number
CS874015A
Other languages
Czech (cs)
Other versions
CS401587A1 (en
Inventor
Milan Hubacek
Vlastimil Brozek
Josef Bronec
Original Assignee
Milan Hubacek
Vlastimil Brozek
Josef Bronec
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Milan Hubacek, Vlastimil Brozek, Josef Bronec filed Critical Milan Hubacek
Priority to CS874015A priority Critical patent/CS260744B1/en
Publication of CS401587A1 publication Critical patent/CS401587A1/en
Publication of CS260744B1 publication Critical patent/CS260744B1/en

Abstract

Řešení se týká keramického materiálu určeného například pro odtrhovací kroužky používané při kontinuálním lití kovů a slitin. Vsázka sestává z 0,012 až 24 °/o hmot. uhlíku, 0,0.11 až 48 % hmot. karbidotvorných prvků ze skupiny zahrnující křemík, bor a titan jednotlivě nebo ve směsi a zbytek tvoří turbostratický nitrid boritý.The solution relates to a ceramic material intended for example for tear-off rings used in continuous casting of metals and alloys. The charge consists of 0.012 to 24 % by weight of carbon, 0.0.11 to 48 % by weight of carbide-forming elements from the group including silicon, boron and titanium individually or in a mixture and the remainder is turbostratic boron nitride.

Description

Vynález se týká vsázky pro výrobu žáruvzdorného keramického1 materiálu.The invention relates to a feedstock for the production of one refractory ceramic material.

Žáruvzdorná keramika na bázi hexagonální nitrid tooritý — karbid karbidotvorných prvků je v současné době připravována tlakovým slinováním, resp. žárovým lisováním, směsi prásků nitridu boritého a karbidu titanu, zirkonia nebo jiného přechodného prvku. V důsledku působení vysokých teplot v procesu tlakového slinování dochází při zhutňování prásku k růstu zrna slinovaného materiálu. Tento růst vede ke snížení mechanických vlastností slinuté keramiky.Refractory ceramics based on hexagonal toorium nitride - carbide carbide forming elements are currently prepared by pressure sintering, respectively. by hot pressing, a mixture of boron nitride and titanium carbide powders, zirconium or other transition element. Due to the effects of high temperatures in the pressure sintering process, the grain of the sintered material grows during compacting the powder. This growth leads to a reduction in the mechanical properties of the sintered ceramic.

Uvedené nevýhody odstraňuje vsázka pro výrobu žáruvzdorné keramiky podle vynálezu. Podstata vynálezu spočívá v tom, že vsázka sestává z 0,012 až 24 % hmot. uhlíku, 0,011 až 48 % hmot. karhidotvorného prvku ze skupiny zahrnující křemík, hor a titan jednotlivě nebo ve směsi tak, aby tato směs byla výhodně v molárním poměru odpovídajícím požadovanému stechiometrickému poměru, zbytek tvoří turbostratický nitrid boritý.These disadvantages are avoided by the charge for the production of the refractory ceramic according to the invention. The invention consists in that the charge consists of 0.012 to 24% by weight. % of carbon, 0.011 to 48 wt. a carburizing element selected from the group consisting of silicon, horium and titanium individually or in a mixture such that the mixture is preferably in a molar ratio corresponding to the desired stoichiometric ratio, the remainder being turbostratic boron nitride.

Při použití vsázky podle vynálezu se zamezuje růstu zrn vstupního· práškového BN během žárového lisování, čímž se dosahuje výborných mechanických vlastností, včetně jejich izotropie, ve srovnání s keramikou připravenou žárovým lisováním směsi nitridu boritého a příslušných karbidů. Přítomnost elementární karbidotvorné látky, která má dobré redukční vlastnosti, zabezpečuje vysokou životnost grafitových lisovacích forem, nebol tato látka vystupuje zároveň jako getr a váže na sebe kyslík obsažený v lisovaném prášku.By using the batch according to the invention, grain growth of the input BN powder is prevented during hot pressing, thereby achieving excellent mechanical properties, including their isotropic, as compared to the ceramic prepared by hot pressing of a mixture of boron nitride and the corresponding carbides. The presence of an elemental carbide former having good reducing properties ensures a long service life of the graphite molds, since it also acts as a getter and binds to it the oxygen contained in the compressed powder.

•Vsázka se připravuje tak, že se smísí a zhomogenizuje turbostratický BN, elementární uhlík jako aktivní uhlí, saze nebo jiná uhlíkatá látka nejlépe s velkým měrným povrchem a prášek elementární 'karbidotvorné látky jako křemík, bor, titan, zirkonlum nebo jiná, eventuálně jejich směs tak, aby tato· směs byla nejlépe v molárním poměru odpovídajícím požadovanému stechiometrickému poměru. Homogenizaci je nejlépe vést v rotačním nebo vibračním kulovém nebo tyčovém mlýně. Dostatečně zhomogenizovaná směs je eventuálně předlisována za studená a potom žárově lisována v grafitové lisovací formě při teplotě 1 600 .až 2 100 °C, výhodně při teplotě 1 750 až 1 950 °C. Lisovací tlak činí 5 až 60 MPa, výhodně 10 až 25 MPa.The charge is prepared by mixing and homogenizing turbostratic BN, elemental carbon such as activated carbon, carbon black or other carbonaceous material preferably with a large surface area, and powder of elemental carbide forming agents such as silicon, boron, titanium, zirconium or other, or a mixture thereof such that the mixture is preferably in a molar ratio corresponding to the desired stoichiometric ratio. Homogenization is best conducted in a rotary or vibrating ball or bar mill. The sufficiently homogenized mixture is optionally cold pre-pressed and then hot-pressed in a graphite die at a temperature of 1600 to 2100 ° C, preferably at a temperature of 1750 to 1950 ° C. The pressing pressure is 5 to 60 MPa, preferably 10 to 25 MPa.

IAND

Příklad 1Example 1

Byla připraven směs skládající se z 94 % hmot. turbostratické formy hexagonálního nitridu boritého, 4,8 % hmot. práškového titanu a 1,2 % hmot. aktivního uhlí. Tato směs byla po dobu šesti hodin homogenizována mletím v rotačním kulovém mlýně. Zhomogenizovaná směs byla vsypána do grafitové lisovací formy a lisována tlakem 10A blend consisting of 94 wt. % turbostratic form of hexagonal boron nitride, 4.8 wt. % titanium powder and 1.2 wt. activated carbon. This mixture was homogenized by rotary ball mill grinding for six hours. The homogenized mixture was poured into a graphite die and pressed at 10

MPa při teplotě 1 800 °C. Výsledky chemické a rtg. difrakční analýzy ukázaly, že byl tímto způsobem připraven keramický materiál obsahující 94 °/o hexagonálního nitridu boritého a 6 % karbidu titaničitého. Velikost zrn BN v takto připravené keramice byla shodná s velikostí zrn vstupního práškového· nitridu boritého.MPa at 1800 ° C. Chemical and X-ray results. diffraction analyzes showed that a ceramic material containing 94% hexagonal boron nitride and 6% titanium carbide was prepared in this way. The BN grain size in the ceramic thus prepared was the same as the boron nitride input powder size.

Příklad 2Example 2

Navážením 89,6 % hmot. turbostratické formy hexagonálního nitridu boritého, 9,2 % hmot. práškového zirkonia a 1,2 % hmot. aktivního uhlí byla připravena směs, která byla po· dobu osmi hodin homogenizována v rotačním kulovém mlýně. Zhomogenizovaná směs byla vsypána do grafitové lisovací formy a lisována při teplotě 1 850 °'C tlakem 14 MPa. Výsledky chemické a strukturální analýzy ukázaly, že touto technologií byl připraven keramický materiál složený z 90 θ/ο hexagonálního nitridu boritého a 10 % karbidu titaničitého. Velikost zrn BN takto připravené keramiky byla shodná s velikostí zrn vstupního práškového nitridu boritého.Weighing 89.6% wt. % turbostratic form of hexagonal boron nitride, 9.2 wt. % zirconium powder and 1.2 wt. activated carbon was prepared and homogenized in a rotary ball mill for eight hours. The homogenized mixture was poured into a graphite die and pressed at a temperature of 1850 ° C under a pressure of 14 MPa. The results of chemical and structural analysis showed that this technology produced a ceramic material composed of 90 θ / ο hexagonal boron nitride and 10% titanium carbide. The BN grain size of the ceramics thus prepared was identical to that of the boron nitride feed powder.

Příklad 3Example 3

Navážením 86 % hmot. turbostratické formy hexagonálního nitridu boritého, 5,6 procent hmot. práškového křemíku, 4,8 % hmot. práškového titanu a 3,6 % hmot. aktivního uhlí byla připravena směs, která byla po dobu dvou hodin homogenizována mletím ve vibračním kulovém mlýně. Zhomogenizovaná směs byla vsypána do grafitové lisovací formy a lisována tlakem 12 MPa při teplotě 1 850 °C. Výsledky chemické ,a difrakční rtg. analýzy ukázaly, že touto technologií byla připravena keramika složená z 86 % hexagonálního nitridu boritého s vysokým stupněm uspořádání krystalové mřížky, 8 % karbidu křemičitého a 6 % karbidu titaničitého. Velikost zrn nitridu boritého byla opět stejná před i po žárovém lisování.Weighing 86% wt. % turbostratic form of hexagonal boron nitride, 5.6 wt. % silicon powder, 4.8 wt. % titanium powder and 3.6 wt. activated carbon was prepared and homogenized for two hours by milling in a vibratory ball mill. The homogenized mixture was poured into a graphite die and pressed at 12 MPa at 1850 ° C. Results of chemical, and diffraction X-ray. analyzes showed that this technology prepared ceramics consisting of 86% hexagonal boron nitride with a high degree of crystal lattice arrangement, 8% silica carbide and 6% titanium carbide. The boron nitride grain size was again the same before and after the hot pressing.

Příklad 4Example 4

Byla připravena směs se složením 82 % hmot. turbostratické formy hexagonálního nitridu boritého, 5,4 % hmot. povrchově aktivního uhlíku, 12,6 % hmot. práškového křemíku. Tato· směs byla po dobu dvou hodin homogenizována ve vibračním kulovém mlýně. Zhomogenizovaná směs byla vsypána do grafitové lisovací formy a lisována tlakem 12 MPa při teplotě 1 850 °C. Výsledky chemické a rtg. difrakční analýzy ukázaly, že tímto způsobem byl připraven kompozitní keramický materiál se složením 82 procent hexagonálního nitridu boritého s plně vyvinutou krystalovou mřížkou a 18 % karbidu křemičitého.A blend of 82 wt. % turbostratic forms of hexagonal boron nitride, 5.4 wt. % surfactant, 12.6 wt. of silicon powder. The mixture was homogenized in a vibrating ball mill for two hours. The homogenized mixture was poured into a graphite die and pressed at 12 MPa at 1850 ° C. Chemical and X-ray results. diffraction analyzes showed that a composite ceramic material of 82 percent hexagonal boron nitride with a fully developed crystal lattice and 18% silica carbide was prepared in this way.

P ř í k 1 a d 5Example 1 a d 5

Smísily se 2 kg kyseliny trihydrogenborité s 4,4 kg močoviny. Směs se zahřála na teplotu 280 °C, doba zahřívání činila šest hodin. Takto vznikl bílý porézní spečenec, který byl tři hodiny mlet v rotačním kulovém mlýně, potom byl vpraven, do křemenné trubice, v níž byl po dobu '2 hodin žíhán v proudu amoniaku o· průtočné rychlosti 1 cm/s při teplotě 700 °C a potom další dvě hodiny při teplotě 1000· °C. Tímto způsobem bylo získáno 580· g turbostratického nitridu boritého obsahujícího· 3,8 % kyslíku a 0,8 % uhlíku. K tomuto materiálu bylo přidáno 10,6 gramu práškového křemíku, směs byla homogenizována po dobu šesti hodin v rotačním kulovém mlýně a potom lisována při teplotě 1 850 °C tlakem 15 MPa v grafitové lisovací formě. Analýza takto připravené keramiky ukázala, že se jedná o hexagonální nitrid boritý obsahující 2,7 % karbidu křemičitého. Porezita takto připravené keramiky činila 4,5 %.2 kg of borohydride were mixed with 4.4 kg of urea. The mixture was heated to 280 ° C for six hours. This resulted in a white porous sinter, which was milled for three hours in a rotary ball mill, then introduced into a quartz tube in which it was annealed in a stream of ammonia at a flow rate of 1 cm / s at 700 ° C for 2 hours. then an additional two hours at 1000 ° C. 580 g of turbostratic boron nitride containing 3.8% oxygen and 0.8% carbon were thus obtained. To this material was added 10.6 grams of silicon powder, the mixture was homogenized for six hours in a rotary ball mill and then compressed at 1850 ° C under a pressure of 15 MPa in a graphite compression mold. Analysis of the ceramics thus prepared showed that it was hexagonal boron nitride containing 2.7% silica carbide. The porosity of the prepared ceramics was 4.5%.

Claims (1)

PŘEDMĚTSUBJECT Vsázka pro výrobu žáruvzdorné keramiky •na bázi hexagonálního nitridu boritého s přísadou karbidů, vyznačující se tím, že sestává z 0,012 až 24 % hmotnostních uhlíku, 0,011 až 48 % hmotnostních karbidotvornéVYNÁLEZU ho prvku ze skupiny zahrnující křemík, bor •a titan jednotlivě nebo ve směsi, přičemž zbytek je tvořen turbostratickým nitridem boritým.A charge for the production of a refractory ceramic based on hexagonal boron nitride with carbide additive characterized in that it consists of 0.012 to 24% by weight of carbon, 0.011 to 48% by weight of a carbide-forming element of the group consisting of silicon, boron and titanium individually or in a mixture wherein the remainder is turbostratic boron nitride.
CS874015A 1987-06-02 1987-06-02 Charge for the production of refractory ceramics CS260744B1 (en)