Prior art keywords
piezoelectric ceramic
ceramic composition
tio
lead
xbicro
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP11150054A
Other languages
English (en)
Other versions
JP4141051B2 (ja
Inventor
Atsushi Sasaki
淳 佐々木
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tokin Corp
Original Assignee
Tokin Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tokin Corp filed Critical Tokin Corp
Priority to JP15005499A priority Critical patent/JP4141051B2/ja
Publication of JP2000335967A publication Critical patent/JP2000335967A/ja
Application granted granted Critical
Publication of JP4141051B2 publication Critical patent/JP4141051B2/ja
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Links

Landscapes

  • Compositions Of Oxide Ceramics (AREA)

Abstract

(57)【要約】 【課題】 無鉛で、高いQmを有する圧電磁器組成物を
提供する。 【解決手段】 一般式(1−X)(Bi0.5Na
0.5)TiO−XBiCrOにおいて、Xを0.
03≦X≦0.3の範囲とする。

Description

【発明の詳細な説明】
【0001】
【発明の属する技術分野】本発明は、波動デバイス、フ
ィルター、共振子等に用いられる圧電磁器組成物に関す
る。
【0002】
【従来の技術】従来、この種の圧電磁器組成物として
は、二成分で構成されるPZT(PbTiO−PbZ
rO)系磁器や三成分で構成されるPCM[PbTi
−PbZrO−Pb(Mg0.5Nb0.5)T
iO]系磁器が主に用いられてきた。その理由として
は、上記の組成物が大きな圧電性を示すことはもちろん
であるが、それとともに、その用途がセンサー、アクチ
ュエーター、フィルター等多種にわたり、各用途に要求
される特性も様々であるのに対し、上記組成系では、各
成分量の割合を調整することにより、要求に対応した特
性に適宜に操作できるからである。
【0003】しかし、これらの組成物は、いずれも鉛を
主成分とするもので、原料比で酸化鉛として60wt%
以上も含まれている。酸化鉛は、低温でも揮発性が高
く、仮焼、焼結等の製造時に揮発したり、また、産業廃
棄物中から溶出することも考えられる。しかし、この対
策をするには、設備設置のため膨大な費用を投じなけれ
ばならない。そこで、無鉛で、大きな圧電特性を示す材
料が要望されている。
【0004】また、既存の無鉛圧電磁器組成物、一般式
(Bi0.5Na0.5)TiOは、機械的品質係数
Qmの値が低く、高いQmが必要とされるフィルター、
共振子等の用途に適用することは困難であった。
【0005】
【発明が解決しようとする課題】本発明は、上記の課題
を解決し、無鉛で、高いQmを有する圧電磁器組成物を
提供することにある。
【0006】
【課題を解決するための手段】本発明は、一般式(1−
X)(Bi0.5Na0.5)TiO−XBiCrO
で表され、Xが0.03≦X≦0.3の範囲であるこ
とを特徴とする圧電磁器組成物である。
【0007】
【発明の実施の形態】主成分原料として、化学的に高純
度であるBi、NaCO、TiO 、Cr
を用いた。これらを一般式(1−X)(Bi0.5
Na0.5)TiO−XBiCrO(0≦X≦0.
4)に対し化学量論的に配合し、ボールミルによりエタ
ノール中で20時間混合した。これを800℃で1時間
保持して仮焼し、次に、10時間粉砕を行った。バイン
ダーとしてポリビニルアルコールを用い造粒し、圧力1
ton/cmで直径20mm、厚さ1mmの円板状に
加圧成形した。焼成は、温度1050〜1150℃で2
時間保持して行った。
【0008】この焼結体の両面に銀電極を設け、100
℃のシリコーンオイル中で直流電圧4kV/mmを電極
間に加え、焼結体を厚み方向に分極した。
【0009】そして、これらの試料について圧電、誘電
特性の測定を行った。圧電特性は、LFインピーダンス
アナライザーを用い、共振−反共振法により電気機械結
合係数k33、kp、kt、機械的品質係数Qmを算出
し、評価した。また、誘電特性は、LCRメータを用い
て周波数1MHzで測定を行い、比誘電率ε33 /ε
で評価した。
【0010】表1に、(1−X)(Bi0.5Na
0.5)TiO−XBiCrOにおいて、0≦X≦
0.4の範囲におけるk33、kp、kt、Qm、及び
ε33 /εを示す。
【0011】
【表1】
【0012】表1において、Qmは、X=0.2で、最
大値1288であり、(Bi0.5Na0.5)TiO
に対し、Qmが顕著に改善していることが確認でき
た。しかし、0.03≦X≦0.3の範囲外では、Qm
が700以下と非常に小さく、実用化は難しいことがわ
かった。
【0013】また、0.03≦X≦0.3の範囲では、
33、kp、ktも増加しており、実用に適している
ことがわかった。
【0014】以上より、(Bi0.5Na0.5)Ti
にBiCrOを3〜30mol%固溶させること
により、(Bi0.5Na0.5)TiOのk33
kp、ktを劣化させることなく、Qmを向上させるこ
とができる。これにより、フィルター、共振子等の用途
への適用が可能となる。
【0015】
【発明の効果】以上説明したように、本発明によれば、
無鉛で、高いQmを有する圧電磁器組成物を提供するこ
とができた。

Claims (1)

    【特許請求の範囲】
  1. 【請求項1】 一般式(1−X)(Bi0.5Na
    0.5)TiO−XBiCrOで表され、Xが0.
    03≦X≦0.3の範囲であることを特徴とする圧電磁
    器組成物。
JP15005499A 1999-05-28 1999-05-28 圧電磁器組成物 Expired - Lifetime JP4141051B2 (ja)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP15005499A JP4141051B2 (ja) 1999-05-28 1999-05-28 圧電磁器組成物

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
JP15005499A JP4141051B2 (ja) 1999-05-28 1999-05-28 圧電磁器組成物

Publications (2)

Publication Number Publication Date
JP2000335967A true JP2000335967A (ja) 2000-12-05
JP4141051B2 JP4141051B2 (ja) 2008-08-27

Family

ID=15488509

Family Applications (1)

Application Number Title Priority Date Filing Date
JP15005499A Expired - Lifetime JP4141051B2 (ja) 1999-05-28 1999-05-28 圧電磁器組成物

Country Status (1)

Country Link
JP (1) JP4141051B2 (ja)

Cited By (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2013179260A (ja) * 2012-01-31 2013-09-09 Tdk Corp 圧電組成物および圧電素子
JP2014209554A (ja) * 2013-03-29 2014-11-06 Tdk株式会社 圧電組成物および圧電素子
CN113198458A (zh) * 2021-04-21 2021-08-03 中国海洋大学 一种铋铬复合氧化物半导体光催化剂及其制备方法和应用

Cited By (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2013179260A (ja) * 2012-01-31 2013-09-09 Tdk Corp 圧電組成物および圧電素子
JP2014209554A (ja) * 2013-03-29 2014-11-06 Tdk株式会社 圧電組成物および圧電素子
CN113198458A (zh) * 2021-04-21 2021-08-03 中国海洋大学 一种铋铬复合氧化物半导体光催化剂及其制备方法和应用

Also Published As

Publication number Publication date
JP4141051B2 (ja) 2008-08-27

Similar Documents

Publication Publication Date Title
JP4510966B2 (ja) 圧電体セラミックス
JP4929522B2 (ja) 圧電磁器組成物
JP3259677B2 (ja) 圧電磁器組成物
JP4513948B2 (ja) 圧電磁器およびその製造方法
JP3259678B2 (ja) 圧電磁器組成物
JP3228175B2 (ja) 圧電磁器組成物
JP4524558B2 (ja) 圧電磁器およびその製造方法
JP2014224038A (ja) 圧電セラミックス及びこれを用いた圧電デバイス
JP4140796B2 (ja) 圧電セラミックス
JP4995412B2 (ja) 圧電磁器組成物及びこれを用いた圧電素子
JPH11171643A (ja) 圧電性磁器組成物
JP4437848B2 (ja) 圧電体磁器組成物
JP3198906B2 (ja) 圧電体磁器組成物
JPH11217262A (ja) 圧電磁器組成物
JP4247936B2 (ja) 圧電体磁器組成物
JP2009012997A (ja) 無鉛圧電磁器組成物
JP2006151796A (ja) 圧電セラミックス組成物
JP4052612B2 (ja) 圧電体磁器組成物
JP2000335967A (ja) 圧電磁器組成物
JP4927378B2 (ja) 圧電磁器組成物および圧電素子
JP2004182532A (ja) 圧電磁器組成物
JP4141052B2 (ja) 圧電磁器組成物
JP3699599B2 (ja) 圧電磁器
JP2001048641A (ja) 圧電磁器組成物
JP4370135B2 (ja) 圧電磁器組成物

Legal Events

Date Code Title Description
A621 Written request for application examination

Free format text: JAPANESE INTERMEDIATE CODE: A621

Effective date: 20051012

A977 Report on retrieval

Free format text: JAPANESE INTERMEDIATE CODE: A971007

Effective date: 20080401

TRDD Decision of grant or rejection written
A01 Written decision to grant a patent or to grant a registration (utility model)

Free format text: JAPANESE INTERMEDIATE CODE: A01

Effective date: 20080528

A01 Written decision to grant a patent or to grant a registration (utility model)

Free format text: JAPANESE INTERMEDIATE CODE: A01

A61 First payment of annual fees (during grant procedure)

Free format text: JAPANESE INTERMEDIATE CODE: A61

Effective date: 20080610

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20110620

Year of fee payment: 3

R150 Certificate of patent or registration of utility model

Free format text: JAPANESE INTERMEDIATE CODE: R150

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20110620

Year of fee payment: 3

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20120620

Year of fee payment: 4

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20120620

Year of fee payment: 4

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20130620

Year of fee payment: 5

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20140620

Year of fee payment: 6

S533 Written request for registration of change of name

Free format text: JAPANESE INTERMEDIATE CODE: R313533

R350 Written notification of registration of transfer

Free format text: JAPANESE INTERMEDIATE CODE: R350

EXPY Cancellation because of completion of term