JP2004262995A - Method for repairing wall of coke oven - Google Patents

Method for repairing wall of coke oven Download PDF

Info

Publication number
JP2004262995A
JP2004262995A JP2003052538A JP2003052538A JP2004262995A JP 2004262995 A JP2004262995 A JP 2004262995A JP 2003052538 A JP2003052538 A JP 2003052538A JP 2003052538 A JP2003052538 A JP 2003052538A JP 2004262995 A JP2004262995 A JP 2004262995A
Authority
JP
Japan
Prior art keywords
repair
coke oven
furnace wall
combustion chamber
sprayed
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP2003052538A
Other languages
Japanese (ja)
Other versions
JP4123975B2 (en
Inventor
Toru Shiozawa
亨 塩沢
Masakatsu Takeshita
将功 竹下
Hitoshi Tanaka
田中  均
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
JFE Steel Corp
Original Assignee
JFE Steel Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by JFE Steel Corp filed Critical JFE Steel Corp
Priority to JP2003052538A priority Critical patent/JP4123975B2/en
Publication of JP2004262995A publication Critical patent/JP2004262995A/en
Application granted granted Critical
Publication of JP4123975B2 publication Critical patent/JP4123975B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

【課題】強固な補修体を簡便且つ確実に形成すると共に、補修効率の向上と補修コストの低減を可能にするコークス炉炉壁の補修方法を提供する。
【解決手段】室炉式コークス炉100の燃焼室120と炭化室110とを仕切る炉壁130の欠損部300において、燃焼室側から前記欠損部と対面する炉壁面へ補修材料320を溶射ランス310で溶射することによって、溶射補修層330を前記欠損部の近傍まで形成した後に、炭化室側から前記欠損部へ補修材料340を溶射して充填する。
【選択図】 図1
An object of the present invention is to provide a method of repairing a coke oven wall, in which a strong repair body is easily and reliably formed, and which can improve repair efficiency and reduce repair cost.
In a coke oven, a repair material is sprayed from a combustion chamber side to a furnace wall facing the defect at a defect portion of a furnace wall that separates a combustion chamber from a combustion chamber. After the sprayed repair layer 330 is formed up to the vicinity of the defect, the repair material 340 is sprayed and filled from the carbonization chamber side to the defect.
[Selection diagram] Fig. 1

Description

【0001】
【発明の属する技術分野】
本発明は、室炉式コークス炉炉壁の補修方法に係り、特にコークス炉の燃焼室と炭化室とを仕切る炉壁に生じた欠損部に対する補修方法に関する。
【0002】
【従来の技術】
室炉式スークス炉100は図4に示すように、石炭が装入される炭化室110と、ガスが燃焼する燃焼室120が交互に配列された設備であり、炭化室110と燃焼室120とは炉壁レンガ130(図5を参照)により仕切られている。
石炭は炭化室110の炉上に設けられた装入口140から装入されて燃焼室120から炉壁レンガ130を介して伝わる熱により昇温、乾留し、コークスへ転換する。この時に発生するコークスガスは上昇管160からドライメーン170に集められ、ガス利用設備へ送られる。生成したコークスは炭化室110の左右に設けられた炉蓋を外した上で一方から押出機180により押し出されて他方に配置した消火電車190へ入れられ、湿式あるいは乾式で冷却されて高炉等での利用に供せられる。
【0003】
また、図5には、室炉式コークス炉の一例であるカールスチル式コークス炉の一部分の平面断面図を示す。燃焼室120は炭化室110へ均一に熱を供給するために、同図に示されるように複数の燃焼ガス流路200に仕切られており、高温の燃焼ガスが流通する。
室炉式コークス炉では生成したコークスを押出機180で押し出すために、炉壁レンガ130の炭化室110側面はコークスとの摩擦等により損耗する恐れがある。また炉壁レンガ130の目地部分210の段差や部分的な傷があると、その部分でコークスが引っかかり、炉壁へ過大な応力が発生して炉壁レンガ130そのものが欠損するといった事態が考えられる。
【0004】
コークス炉の炉壁補修に関しては、特許文献1において、炉壁面の摩耗や剥離といった損傷部に補修材料を熱間で吹き付ける炉壁補修方法が開示されている。また、特許文献2に開示されているように、損傷個所のある炉壁レンガを含むレンガを一体として新規のレンガと積み替える炉壁補修方法も提案されている。
【0005】
【特許文献1】
特開平9−210567号公報
【特許文献2】
特開2001−19968号公報
【0006】
【発明が解決しようとする課題】
しかしながら、これら従来の補修方法にあっては、以下の問題点があった。
即ち、特許文献1に開示された技術は、炉壁面の摩耗や剥離といった部分的な損傷については効果的であるが、炉壁レンガが欠損して炭化室と燃焼室が連通してしまった場合には、図6に示すように炉壁レンガの厚み約100mmを炭化室側から溶射補修材で埋める必要があるが、燃焼室側からの吹付けで欠損部を均質に補修することが困難であるため、補修部分の強度が十分得られず、使用中に再度損傷し易いという問題があった。
【0007】
また、特許文献2に開示された補修方法は、広範囲にわたって健全なレンガ補修体を施工することで新規コークス炉と同等の炉壁を形成することができるが、レンガを広範囲に解体し、積み直すために、多大な時間がかかり、補修効率が悪化し、補修コストが嵩む場合があった。
そこで、本発明は、上述の問題点に鑑みてなされたものであり、欠損部に応じて強固な補修体を簡便且つ確実に形成すると共に、補修効率の向上と補修コストの低減を可能にするコークス炉の補修方法を提供することを課題とする。
【0008】
【課題を解決するための手段】
上記課題を解決するため、本発明の請求項1は、コークス炉の燃焼室と炭化室とを仕切る炉壁の欠損部において、燃焼室側から前記欠損部と対面する炉壁面へ補修材料を溶射することによって、溶射補修層を前記欠損部の近傍まで形成した後に、炭化室側から前記欠損部へ補修材料を溶射して充填することを特徴とするコークス炉炉壁の補修方法である。
さらに、本発明の請求項2は、前記溶射補修層は、燃焼室上部から挿入された溶射ランスによって補修材料を溶射して形成されたことを特徴とする請求項1に記載のコークス炉炉壁の補修方法である。
【0009】
【発明の実施の形態】
以下、本発明の好ましい実施の形態を図面に基づいて説明する。図1は室炉式コークス炉の炉壁レンガの一部に欠損部が生じた場合を示す一部分の断面模式図であり、図2と図3は図1の一部分を拡大するものであり、本発明に係るコークス炉炉壁の補修方法を説明する模式図である。
【0010】
図1と図2に示すように、室炉式コークス炉100の炭化室110と燃焼室120とを仕切る炉壁レンガ130においては、炭化室110と燃焼室120までを連通するような大きな欠損部300が生じたときに、当該欠損部300のある燃焼室120における炉上部のピンホール150から、補修材料320を溶射するための溶射ランス310(図2を参照)を挿入し、前記欠損部300と対向する炉壁レンガ面に対して補修材料320を溶射する。
【0011】
この際に、図3に示すように、溶射補修層330を盛り上げていって盛り上げた頂部が前記欠損部300の近傍となるまで、燃焼室120内部での溶射を実施する。
その後、当該欠損部300の炭化室110側から欠損部300へ向けて、補修材料340の溶射を行う。この際、炭化室110側から見て欠損部300の奥に燃焼室120側に設けた溶射補修層330の頂部を観察できるので、この頂部と欠損部300の周囲の炉壁レンガ300とを補修材料で架橋するように溶射補修を行い、欠損部内部全体に補修材料が充填されるように溶射を行う。
【0012】
なお、溶射に用いる補修材料320、340は通常のコークス炉の炉壁の溶射補修に用いられる材料を適宜用いればよく、SiO2、Al2O3、コージエライトやそれらの混合物あるいは金属Si、金属Al等金属成分を含む補修材料等、補修の対象とする炉壁の材質、補修部位等に応じて選択すればよい。
【0013】
【実施例】
以下、図1乃至図3を参照して本発明の実施例について説明する。
本実施例は、炭化室を102門有する日産能力3350tの室炉式コークス炉の炉壁の一部において、100mm×700mmの範囲で炭化室と燃焼室とを連通する欠損が生じた場合について、本発明の効果を検討した。
【0014】
先ず燃焼室120側に、欠損部300に対向する炉壁面から溶射補修層330を盛り上げて欠損部300の存する炉壁面から50mmの位置にまで溶射を行った。その後に、当該欠損部300の炭化室110側から溶射補修層330への溶射を行って欠損部300との間に溶射補修層330を架橋し、最終的に欠損部全体を溶射補修層330で埋めて補修した。
【0015】
なお、この補修にあたっては、欠損部300のある炉壁面に隣接する炭化室110を含め、両隣の炭化室110の操業を停止し、冷却から、補修、再加熱を行って通常の操業を再開するまでに、5日間要した。この補修により、当該炭化室の使用再開後1年を経過しても、当該欠損部における補修材料の剥離、欠損は生じなかった。
【0016】
一方、このような欠損部が発生したときに、従来行っていた炭化室側から欠損部のレンガ側面へ向けて溶射補修材を溶射する補修方法を行った場合には、補修にあたり本発明と同様に5日間程度の操業停止を必要とするが、その補修後半年程度で溶射補修材の剥離等が生じて再補修を行うのがほとんどであったのに比べて、補修頻度が格段に低減することができた。この場合も補修コストは本発明と同程度であった。
【0017】
また、前記欠損部の補修のために、当該部分のレンガを積み替える補修を行った場合、特許文献2に示されるような補修部分を含むレンガをフロック化して効率的に補修した場合であっても、停止期間として2週間程度必要であり、設備稼働率がより悪化することとなった。また、補修コストも1箇所あたり本願発明に比べて約20倍近くに及び、非常に高価なものとなる。
【0018】
【発明の効果】
以上説明したように、本発明に係るコークス炉炉壁の補修方法は、燃焼室側から欠損部と対面する炉壁面から溶射補修層を前記欠損部の近傍まで盛り上げた後に、炭化室側から前記欠損部への溶射を行うことにより、室炉式コークス炉の炭化室と燃焼室を連通して発生した大きな損傷に対しても、簡便且つ確実に補修体を形成することができるとともに、補修効率の向上と補修コストの低減が可能となる。
【図面の簡単な説明】
【図1】室炉式コークス炉の炉壁レンガの一部に欠損部が生じた場合を示す一部分の断面模式図。
【図2】図1の一部分を拡大するもので、本発明に係るコークス炉炉壁の補修方法を説明する模式図である。
【図3】図1の一部分を拡大するもので、本発明に係るコークス炉炉壁の補修方法を説明する模式図である。
【図4】室炉式コークス炉の全体斜視概念図である。
【図5】カールスチル式コークス炉の一部の水平断面図である。
【図6】従来の炉壁吹付け補修方法による欠損部の補修状態を示す模式図である。
【符号の説明】
100 室炉式コークス炉
110 炭化室
120 燃焼室
130 炉壁レンガ
140 装入口
150 ピンホール
200 燃焼ガス流路
300 欠損部
310 溶射ランス
320 補修材料
330 溶射補修層
340 補修材料
[0001]
TECHNICAL FIELD OF THE INVENTION
The present invention relates to a method for repairing a coke oven wall of a chamber furnace type coke oven, and more particularly to a method for repairing a chipped portion generated in a furnace wall separating a combustion chamber and a carbonization chamber of a coke oven.
[0002]
[Prior art]
As shown in FIG. 4, the chamber furnace type soot furnace 100 is a facility in which a coking chamber 110 in which coal is charged and a combustion chamber 120 in which gas is burned are alternately arranged. Are separated by furnace wall bricks 130 (see FIG. 5).
The coal is charged from a charging port 140 provided on the furnace of the carbonization chamber 110, heated by the heat transmitted from the combustion chamber 120 through the furnace wall brick 130, carbonized, and converted into coke. The coke gas generated at this time is collected from the riser 160 into the dry main 170 and sent to the gas utilization facility. The generated coke is extruded by an extruder 180 from one side after being removed from the furnace lids provided on the left and right sides of the carbonization chamber 110, is put into a fire extinguishing train 190 arranged on the other side, is cooled in a wet or dry system, and is cooled in a blast furnace or the like. To be used.
[0003]
FIG. 5 is a plan cross-sectional view of a part of a Carlstil type coke oven which is an example of a chamber oven type coke oven. The combustion chamber 120 is partitioned into a plurality of combustion gas channels 200 as shown in FIG. 1 to uniformly supply heat to the carbonization chamber 110, and a high-temperature combustion gas flows.
In the coke oven type coke oven, since the generated coke is extruded by the extruder 180, the side surface of the coking chamber 110 of the oven wall brick 130 may be worn due to friction with the coke. Further, if there is a step or a partial scratch at the joint portion 210 of the furnace wall brick 130, coke is caught at that portion, and excessive stress is generated on the furnace wall, and the furnace wall brick 130 itself may be damaged. .
[0004]
Regarding furnace wall repair of a coke oven, Patent Literature 1 discloses a furnace wall repair method in which a repair material is hot-sprayed on a damaged portion such as abrasion or peeling of a furnace wall. Further, as disclosed in Patent Document 2, a method of repairing a furnace wall has been proposed in which bricks including a furnace wall brick having a damaged portion are integrally transferred to new bricks.
[0005]
[Patent Document 1]
JP-A-9-210567 [Patent Document 2]
JP 2001-19968 A
[Problems to be solved by the invention]
However, these conventional repair methods have the following problems.
That is, the technique disclosed in Patent Document 1 is effective for partial damage such as wear and peeling of the furnace wall, but when the furnace wall brick is lost and the carbonization chamber and the combustion chamber communicate with each other. As shown in FIG. 6, it is necessary to fill the furnace wall brick with a thickness of about 100 mm with the thermal spray repair material from the carbonization chamber side as shown in FIG. 6, but it is difficult to uniformly repair the defective portion by spraying from the combustion chamber side. Therefore, there is a problem that the strength of the repaired portion cannot be sufficiently obtained, and the portion is easily damaged again during use.
[0007]
In addition, the repair method disclosed in Patent Document 2 can form a furnace wall equivalent to that of a new coke oven by constructing a healthy brick repair body over a wide range, but dismantle and reload bricks over a wide range. Therefore, it takes a lot of time, the repair efficiency is deteriorated, and the repair cost is sometimes increased.
In view of the above, the present invention has been made in view of the above-described problems, and enables to easily and surely form a strong repair body according to a defect portion, and to improve repair efficiency and reduce repair cost. An object of the present invention is to provide a method for repairing a coke oven.
[0008]
[Means for Solving the Problems]
In order to solve the above-mentioned problem, a first aspect of the present invention is to spray a repair material from a combustion chamber side to a furnace wall facing the defective part in a defective part of a furnace wall separating a combustion chamber and a carbonization chamber of a coke oven. A method for repairing a coke oven wall, comprising: forming a sprayed repair layer up to the vicinity of the defective portion, and then spraying and filling a repair material from the carbonization chamber side to the defective portion.
Further, the coke oven wall according to claim 1, wherein the thermal spray repair layer is formed by thermal spraying the repair material by a thermal spray lance inserted from above the combustion chamber. Repair method.
[0009]
BEST MODE FOR CARRYING OUT THE INVENTION
Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings. FIG. 1 is a schematic cross-sectional view of a part of a furnace wall brick of a coke oven furnace in which a part of a wall brick has a defect, and FIGS. 2 and 3 are enlarged views of a part of FIG. It is a mimetic diagram explaining the repair method of the coke oven wall concerning the invention.
[0010]
As shown in FIGS. 1 and 2, in a furnace wall brick 130 that partitions a coking chamber 110 and a combustion chamber 120 of a coke oven type coke oven 100, a large defective portion communicating with the coking chamber 110 and the combustion chamber 120 is provided. When 300 occurs, a thermal spray lance 310 (see FIG. 2) for thermal spraying the repair material 320 is inserted from a pinhole 150 at the upper part of the furnace in the combustion chamber 120 where the defective portion 300 is located. The repair material 320 is sprayed on the furnace wall brick surface opposite to the above.
[0011]
At this time, as shown in FIG. 3, the thermal spraying repair layer 330 is raised and the thermal spraying is performed inside the combustion chamber 120 until the raised top is near the defective portion 300.
Thereafter, the repair material 340 is thermally sprayed from the carbonization chamber 110 side of the defective portion 300 toward the defective portion 300. At this time, since the top of the sprayed repair layer 330 provided on the combustion chamber 120 side can be observed behind the defect 300 when viewed from the carbonization chamber 110 side, the top and the furnace wall brick 300 around the defect 300 are repaired. Thermal spray repair is performed so that the material is crosslinked, and thermal spraying is performed so that the repair material fills the entire inside of the defect.
[0012]
As the repair materials 320 and 340 used for thermal spraying, materials used for thermal spray repair of a furnace wall of a normal coke oven may be appropriately used, and SiO 2 , Al 2 O 3 , cordierite, a mixture thereof, metal Si, metal Al What is necessary is just to select according to the material of the furnace wall to be repaired, the repair site, etc., such as the repair material containing the equal metal component.
[0013]
【Example】
Hereinafter, an embodiment of the present invention will be described with reference to FIGS.
In the present embodiment, in a part of the furnace wall of a coke oven type furnace having a daily production capacity of 3350 t having 102 carbonization chambers, a case occurs in which the communication between the carbonization chamber and the combustion chamber in a range of 100 mm × 700 mm occurs. The effects of the present invention were studied.
[0014]
First, on the combustion chamber 120 side, the thermal spray repair layer 330 was raised from the furnace wall facing the defect 300, and spraying was performed to a position 50 mm from the furnace wall where the defect 300 exists. Thereafter, the sprayed repair layer 330 is bridged between the defective portion 300 and the sprayed repair layer 330 by spraying from the carbonization chamber 110 side of the defective portion 300, and finally the entire defective portion is sprayed with the thermal spray repair layer 330. Filled and repaired.
[0015]
In this repair, the operation of the carbonization chambers 110 on both sides, including the carbonization chamber 110 adjacent to the furnace wall having the defective portion 300, is stopped, and the cooling, repair, reheating, and normal operation are resumed. It took five days to complete. As a result of this repair, even after one year from the resumption of use of the carbonization chamber, the repair material did not peel off or break at the defective portion.
[0016]
On the other hand, when such a defective portion is generated, when a repairing method of spraying a thermal spray repair material from the carbonization chamber side toward the brick side surface of the defective portion, which has been conventionally performed, is performed similarly to the present invention for repair. Requires about five days of operation stoppage, but in the latter half of the repair, the thermal spray repair material peels off, etc., and most repairs are performed. I was able to. Also in this case, the repair cost was almost the same as that of the present invention.
[0017]
In addition, in the case where repair for replacing the bricks of the relevant portion is performed for repairing the defective portion, bricks including the repaired portion as shown in Patent Document 2 are flocculated and efficiently repaired. However, the suspension period required about two weeks, and the equipment operation rate was further deteriorated. In addition, the repair cost is about 20 times as large as that of the present invention per location, which is very expensive.
[0018]
【The invention's effect】
As described above, the method for repairing a coke oven wall according to the present invention includes, after raising the sprayed repair layer from the combustion chamber side to the vicinity of the defective portion from the furnace wall facing the defective portion, the method further comprises: By performing thermal spraying on the defective part, it is possible to easily and reliably form a repair body even for large damage caused by connecting the carbonization chamber and the combustion chamber of the chamber furnace type coke oven, and the repair efficiency And repair costs can be reduced.
[Brief description of the drawings]
FIG. 1 is a schematic cross-sectional view of a part of a furnace coke oven in which a part of a furnace wall brick has a defect.
FIG. 2 is an enlarged view of a part of FIG. 1 and is a schematic diagram illustrating a method of repairing a coke oven wall according to the present invention.
FIG. 3 is an enlarged view of a part of FIG. 1 and is a schematic diagram illustrating a method of repairing a coke oven wall according to the present invention.
FIG. 4 is an overall perspective conceptual view of a chamber coke oven.
FIG. 5 is a horizontal sectional view of a part of the Carl still coke oven.
FIG. 6 is a schematic view showing a repaired state of a defective portion by a conventional furnace wall spraying repair method.
[Explanation of symbols]
100 chamber type coke oven 110 carbonization chamber 120 combustion chamber 130 furnace wall brick 140 inlet 150 pinhole 200 combustion gas flow path 300 chipped portion 310 spray lance 320 repair material 330 thermal spray repair layer 340 repair material

Claims (2)

コークス炉の燃焼室と炭化室とを仕切る炉壁の欠損部において、燃焼室側から前記欠損部と対面する炉壁面へ補修材料を溶射することによって、溶射補修層を前記欠損部の近傍まで形成した後に、炭化室側から前記欠損部へ補修材料を溶射して充填することを特徴とするコークス炉炉壁の補修方法。In the defective part of the furnace wall that separates the combustion chamber and the carbonization chamber of the coke oven, the sprayed repair material is sprayed from the combustion chamber side to the furnace wall facing the defective part to form a thermal spray repair layer up to the vicinity of the defective part. And repairing the coke oven wall by spraying and filling a repair material from the carbonization chamber side to the defective portion. 前記溶射補修層は、燃焼室上部から挿入された溶射ランスによって補修材料を溶射して形成されたことを特徴とする請求項1に記載のコークス炉炉壁の補修方法。The coke oven wall repair method according to claim 1, wherein the thermal spray repair layer is formed by thermal spraying a repair material with a thermal spray lance inserted from above the combustion chamber.
JP2003052538A 2003-02-28 2003-02-28 Coke oven wall repair method Expired - Fee Related JP4123975B2 (en)