JPH01200931A - Polypropylene resin foamed sheet having good heat moldability and preparation thereof - Google Patents
Polypropylene resin foamed sheet having good heat moldability and preparation thereofInfo
- Publication number
- JPH01200931A JPH01200931A JP63258889A JP25888988A JPH01200931A JP H01200931 A JPH01200931 A JP H01200931A JP 63258889 A JP63258889 A JP 63258889A JP 25888988 A JP25888988 A JP 25888988A JP H01200931 A JPH01200931 A JP H01200931A
- Authority
- JP
- Japan
- Prior art keywords
- polypropylene resin
- sheet
- foam sheet
- diameter
- annular
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
Description
【発明の詳細な説明】
(産業上の利用分野)
本発明は、無機質微粉末が多量に混合された熱成形性に
適したポリプロピレン系樹脂発泡シート及びその製造方
法に関し、更に詳細には深絞り成形性が優れ且つ印刷さ
れた所定図形に対する位置ズレの少ない位置合せ成形性
が良いポリプロピレン系樹脂発泡シート及びその製造方
法に関する。Detailed Description of the Invention (Field of Industrial Application) The present invention relates to a polypropylene resin foam sheet containing a large amount of inorganic fine powder and suitable for thermoformability, and a method for producing the same, and more specifically to a method for producing the same. The present invention relates to a polypropylene resin foam sheet that has excellent moldability and has good alignment moldability with little misalignment with respect to a printed predetermined figure, and a method for manufacturing the same.
(従来の技術)
従来、ポリスチレン系樹脂に多量の無機質微粉末が混合
された熱成形性の良いポリスチレン系樹脂発泡シートは
、特開昭58−196239号公報(usp4.426
,065号)に記載されるように公知である。しかし、
このポリスチレン系樹脂発泡シートから成形されたトレ
ー、容器等は耐熱性、耐油性が劣るので電子レンジには
使用できず、深絞りコツプ等の深絞り形状を有する成形
品の成形には不適当であり、更に、耐衝撃性、引張り強
度に弱い材料である。(Prior Art) Conventionally, a polystyrene resin foam sheet with good thermoformability, which is a polystyrene resin mixed with a large amount of inorganic fine powder, has been disclosed in Japanese Patent Application Laid-open No. 196239 (USP 4.426).
, No. 065). but,
Trays, containers, etc. molded from polystyrene resin foam sheets have poor heat resistance and oil resistance, so they cannot be used in microwave ovens, and are unsuitable for molding molded products with deep drawing shapes such as deep drawing cups. Moreover, it is a material with weak impact resistance and tensile strength.
他方、ポリプロピレン系樹脂に多量の無機質微粉末が混
合された熱成形性の良いポリプロピレン系樹脂発泡シー
トは、特開昭60−141728号公報に記載されるよ
うに知られている。このポリプロピレン系樹脂発泡シー
トは、電子レンジに使用される耐熱性、または深絞り成
形性の点で改良されているが、表面に所定の図形、模様
、デザインが印刷された発泡シートを熱成形する場合、
これらの所定の図形等の位置が成形毎に相違するとか、
図形等が成形毎に変形するという問題があった。また、
発泡シートの押出における円筒ドラムでの引取工程で抵
抗が生じて引取スピードが遅く、引きちぎれるという問
題もあった。On the other hand, a foamed polypropylene resin sheet with good thermoformability, which is a mixture of a polypropylene resin and a large amount of inorganic fine powder, is known as described in JP-A-60-141728. This polypropylene resin foam sheet has been improved in terms of heat resistance and deep drawability for use in microwave ovens, but the foam sheet is thermoformed with predetermined shapes, patterns, and designs printed on its surface. case,
The position of these predetermined figures etc. may be different for each molding,
There was a problem that the figures etc. were deformed each time they were molded. Also,
During the extrusion of the foam sheet, resistance was generated during the drawing process using a cylindrical drum, resulting in slow drawing speed and the problem of tearing.
(発明が解決しようとする’K1題)
この発明は、かかる従来の技術的課題を解決し熱成形性
に好適なポリプロピレン系樹脂発泡シートを提供しよう
と種々検討した結果、本発明を完成したもので、本発明
の目的は、熱成形性に好適なポリプロピレン系樹脂発泡
シートを提供するものである。この熱成形性として、深
絞り成形性、複雑な形状の型の出に優れたポリプロピレ
ン系樹脂発泡シートを提供するものであり、特に熱成形
の際、印刷されている所定の図形、模様、デザインの位
置ずれの少ないこれら図形等の変形の小さいポリプロピ
レン系樹脂発泡シートを提供するものである。(K1 problem to be solved by the invention) This invention was completed as a result of various studies aimed at solving the conventional technical problems and providing a polypropylene resin foam sheet suitable for thermoformability. An object of the present invention is to provide a foamed polypropylene resin sheet suitable for thermoformability. This thermoforming property provides a polypropylene resin foam sheet with excellent deep drawability and ability to form molds into complex shapes. The object of the present invention is to provide a polypropylene resin foam sheet in which the positional displacement of the shapes is small and the deformation of these figures is small.
また、この発明の他の目的はポリスチレン系樹脂発泡シ
ートに比較して耐熱性、耐油性に優れたポリプロピレン
系樹脂発泡シートを提供するものである。これにより、
電子レンジにも使用できる耐熱性食品容器が提供できる
。Another object of the present invention is to provide a polypropylene resin foam sheet that has superior heat resistance and oil resistance compared to polystyrene resin foam sheets. This results in
A heat-resistant food container that can also be used in a microwave oven can be provided.
また、この発明のその他の目的は、ポリスチレン系樹脂
発泡シートに比較して、耐衝撃性が良く、柔軟で引張り
強度、曲げ強度の強いポリプロピレン系樹脂発泡シート
を提供するものである。Another object of the present invention is to provide a polypropylene resin foam sheet that has better impact resistance, flexibility, and higher tensile strength and bending strength than polystyrene resin foam sheets.
また、この発明の他の目的は、印刷特性の良いポリプロ
ピレン系樹脂発泡シートを提供するものであり、また使
用後の廃棄物の燃焼カロリーの少ないポリプロピレン系
樹脂発泡シートを提供するものである。Another object of the present invention is to provide a foamed polypropylene resin sheet with good printing properties, and a foamed polypropylene resin sheet that burns less calories from waste after use.
また、この発明の別の目的は、上記ポリプロピレン系樹
脂発泡シートの引取り抵抗を少なくして有利な連続的な
製造方法を提供するものである。Another object of the present invention is to provide an advantageous continuous manufacturing method by reducing the pulling resistance of the polypropylene resin foam sheet.
また、この発明の他の別の目的は、上記ポリプロピレン
系樹脂発泡シートの連続操作性の良い製造方法を提供す
るものである。Another object of the present invention is to provide a method for producing the polypropylene resin foam sheet with good continuous operability.
而して、発明者等は種々研究及び開発を重ねた結果、ポ
リプロピレン系樹脂に無機質微粉末を多量に混合し、か
つ特定の厚み、密度を制御し、押出方向の縦及び横方行
の収縮率のバランスを取ることにより、また、円筒ドラ
ムに段差を設けることにより、前記目的を達成できるこ
とを見出し、この発明を完成した。As a result of various research and development, the inventors mixed a large amount of inorganic fine powder into polypropylene resin, controlled a specific thickness and density, and achieved shrinkage in the longitudinal and transverse directions of extrusion. It was discovered that the above object could be achieved by balancing the ratio and by providing a step on the cylindrical drum, and the present invention was completed.
(課題を解決するため手段)
即ち、この発明の要旨は、ポリプロピレン系樹脂に無機
質微粉末が10〜50重量%均質に混合された、密度0
.2−1.2 g /(!+?、厚さ0.2−3onの
押出発泡シートであって、190℃の雰囲気中で30分
間加熱した場合のタテ及びヨコ方向の収縮率がそれぞれ
5〜30%の範囲にあり、且つヨコの残存率とタテの残
存率の比がl:o、7〜1:1.1であることを特徴と
する熱成形性の良いポリプロピレン系樹脂発泡シートで
ある。(Means for Solving the Problems) That is, the gist of the present invention is to provide a polypropylene resin with a density of 0, in which 10 to 50% by weight of inorganic fine powder is homogeneously mixed.
.. 2-1.2 g/(!+?, extruded foam sheet with a thickness of 0.2-3 on, the shrinkage rate in the vertical and horizontal directions when heated for 30 minutes in an atmosphere of 190 ° C. A polypropylene resin foam sheet with good thermoformability, which is in the range of 30% and has a ratio of horizontal residual rate to vertical residual rate of l:o, 7 to 1:1.1. .
そして、また、該成形性の良いポリプロピレン系樹脂発
泡シートを製造する方法として、ポリプロピレン系樹脂
に無機質微粉末と発泡剤を均質に混合せしめて押出発泡
せしめる方法において、該樹脂に対して10〜50重量
2の無機質微粉末を混合せしめ、押出機先端に装置した
円環状細隙を有する口金から押出し発泡させ、該円環状
ポリプロピレン系樹脂発泡シートを上記円環状細隙の径
の2.0〜3.0倍の径を持つ円筒形ドラムに沿わせて
冷却しながら引き取ることを特徴とする製造方法である
。And, as a method for producing the polypropylene resin foam sheet with good moldability, a method of homogeneously mixing inorganic fine powder and a foaming agent with a polypropylene resin and extrusion foaming is performed. A fine inorganic powder having a weight of 2 is mixed and extruded and foamed through a nozzle having an annular slit installed at the tip of an extruder, and the annular polypropylene resin foam sheet is formed into a foam sheet with a diameter of 2.0 to 3 of the diameter of the annular slit. This manufacturing method is characterized by taking the product along a cylindrical drum having a diameter of 0.0 times while cooling it.
以下、本発明について、詳細に説明する。Hereinafter, the present invention will be explained in detail.
本発明におけるポリプロピレン系樹脂としては、プロピ
レン単独重合体、プロピレン−エチレン共重合体、プロ
ピレン−エチレン−ジエン共重合体等のポリプロピレン
を主とする重合体が用いられる。As the polypropylene resin in the present invention, a polymer mainly composed of polypropylene such as a propylene homopolymer, a propylene-ethylene copolymer, a propylene-ethylene-diene copolymer, etc. is used.
プロピレン単独重合体の融点は176℃であり、共重合
体の融点は135℃〜160℃である。耐熱性の良い発
泡シートにするためには、融点の高いものを用いること
が好ましい。The propylene homopolymer has a melting point of 176°C, and the copolymer has a melting point of 135°C to 160°C. In order to make a foamed sheet with good heat resistance, it is preferable to use a material with a high melting point.
また、ポリプロピレン系樹脂を主成分として、他のポリ
プロピレン、エチレン−酢酸ビニル共重合体等の混和可
能な樹脂を混合できる。Further, with the polypropylene resin as the main component, other miscible resins such as polypropylene and ethylene-vinyl acetate copolymer can be mixed.
無機質微粉末としては、シリカ、ケイ藻土、アルミナ、
酸化チタン、酸化鉄、酸化亜鉛、酸化マグネシウム、軽
石粒等の酸化物、水酸化アルミニウム、水酸化マグネシ
ウム、水酸化マグネシウム、塩基性炭酸マグネシウム等
の水酸化物、炭酸カルシウム、炭酸マグネシウム、ドロ
マイト等の炭酸塩、a酸カルシウム、硫酸バリウム、亜
a酸カルシウム等の硫酸塩、タルク、クレー、アスベス
ト。Inorganic fine powders include silica, diatomaceous earth, alumina,
Oxides such as titanium oxide, iron oxide, zinc oxide, magnesium oxide, pumice grains, hydroxides such as aluminum hydroxide, magnesium hydroxide, magnesium hydroxide, basic magnesium carbonate, calcium carbonate, magnesium carbonate, dolomite, etc. Carbonates, sulfates such as calcium acetate, barium sulfate, and calcium acetate, talc, clay, and asbestos.
ケイ酸カルシウム、モンモリロナイト、ベントナイト等
のケイ酸塩、アルミニウム、鉄、fl鉛等の金属の粉末
を用いることができる。これらを単独又は混合して用い
ることもできるが、特に平均粒径が1〜30ミクロンの
タルク、炭酸カルシウム、クレー、シリカ及びアルミナ
が好適である。Silicates such as calcium silicate, montmorillonite, and bentonite, powders of metals such as aluminum, iron, and fl lead can be used. Although these can be used alone or in combination, talc, calcium carbonate, clay, silica, and alumina having an average particle size of 1 to 30 microns are particularly suitable.
無機質微粉末の量が、樹脂に対して10重量2未満では
、成形品の型の出が悪く、複雑な形状の成形ができない
し、又、燃焼カロリーの上昇が生ずる。一方、50重量
%を越えると、伸びが悪くなり、深絞り成形ができない
と共に耐衝撃性、ヒンジ強度が劣り、発泡シート表面の
外観が悪くなり印刷性が劣る。If the amount of the inorganic fine powder is less than 10 parts by weight based on the resin, the molded product will not come out well, complex shapes cannot be molded, and the burned calories will increase. On the other hand, if it exceeds 50% by weight, elongation becomes poor, deep drawing is not possible, impact resistance and hinge strength are poor, the appearance of the foam sheet surface is poor, and printability is poor.
無機質微粉末は、ポリプロピレン系樹脂に対して10〜
50重量%、好ましくは20〜40重量%均質に混合分
散する必要があり、樹脂と無機粉末の相溶性を良くする
ために一般に用いられているシラン系、チタン系のカッ
プリング剤や分散を良くするための各種界面活性剤、金
属石鹸、多価アルコール、酸無水物等を少量添加するの
が良い。The inorganic fine powder is 10 to 10% of the polypropylene resin.
It is necessary to homogeneously mix and disperse 50% by weight, preferably 20 to 40% by weight, and to improve the compatibility between the resin and the inorganic powder, it is necessary to use a silane-based or titanium-based coupling agent or a dispersion agent that is generally used to improve the compatibility between the resin and the inorganic powder. It is recommended to add small amounts of various surfactants, metal soaps, polyhydric alcohols, acid anhydrides, etc.
このように、この発泡シートには無機物微粉末が多量に
混合されているので、使用後の廃棄物の燃焼カロリーが
低下しており、燃焼処理がしやすく、又発泡シートの単
価を低減できるメリットもある。In this way, this foam sheet contains a large amount of inorganic fine powder mixed in, which reduces the amount of calories burned from waste after use, making it easier to burn and process, and also has the advantage of reducing the unit price of the foam sheet. There is also.
発泡剤としては、常温で気体の窒素ガス、炭酸ガス、空
気又は揮発性発泡剤の水、アルコール、プロパン、ブタ
ン、ペンタン、フレオン11.12゜114、メチルク
ロライド、エチルクロライド等が樹脂に対して0.5〜
5重量%が混合される。また、加熱により分解する化学
発泡剤として、アゾジカルボンアミド、N、N’−ジニ
トロ・ノベンタメチレンテトラミン、P、P’−オキシ
ビス(ベンゼンスルホニルヒドラジド)、p、p’−オ
キシビス(ベンゼンスルホニルカルバジド)、アゾビス
イ・ノブチロニトリル、ベンゼンスルホンヒドラジド、
炭酸水素ナトリウムとクエン酸等が0.5〜5重量%が
混合される。As blowing agents, nitrogen gas, carbon dioxide gas, air, which are gases at room temperature, or volatile blowing agents such as water, alcohol, propane, butane, pentane, Freon 11.12゜114, methyl chloride, ethyl chloride, etc. are used for resins. 0.5~
5% by weight is mixed. In addition, chemical blowing agents that decompose by heating include azodicarbonamide, N,N'-dinitro noventamethylenetetramine, P,P'-oxybis(benzenesulfonylhydrazide), p,p'-oxybis(benzenesulfonylcarbazide). , azobisui-butyronitrile, benzenesulfone hydrazide,
0.5 to 5% by weight of sodium hydrogen carbonate and citric acid are mixed.
そして、この発泡シートの製造には、発泡剤の混合され
る量も比較的少量の0.5〜2重量ででもよく、また成
層圏のオゾン層を破壊しない炭化水素系・熱分解型の発
泡剤の選択も容易である。In the production of this foam sheet, the amount of foaming agent mixed may be relatively small, 0.5 to 2 weight, and the foaming agent may be a hydrocarbon-based or pyrolytic foaming agent that does not destroy the ozone layer in the stratosphere. The selection is also easy.
この発明の発泡シートは一般に押出機を使用して連続的
に製造される。押出機にポリプロピレン系樹脂を供給し
、発泡剤と共に加熱溶融するか、又は押出機の途中から
発泡剤を供給して、よく混練し、発泡適性温度に調整し
て口金に供給される。The foamed sheets of this invention are generally manufactured continuously using an extruder. A polypropylene resin is supplied to an extruder and heated and melted together with a foaming agent, or a foaming agent is supplied from the middle of the extruder, kneaded well, adjusted to a temperature suitable for foaming, and then supplied to a die.
口金への樹脂温度としては、180℃〜240℃に調整
され、口金の温度は、それより10〜60℃低めに設定
される。口金としては、コートハンガータイプやTダイ
タイプの先端の厚さに比べて巾の大きな細隙を有するも
のや、円筒状をしており先端に円環状の細隙を有するも
のが用いられる。前者の口金を用いた場合は、口金から
出た樹脂をロールで冷却し、引取スピード、応力でタテ
方向の延伸量を調整し、更に必要に応じてヨコ方向から
クランプして延伸し、ヨコ方向の延伸を調整する。後者
の口金を用いた場合は円環状の細隙から出た発泡樹脂を
噴出気体により強制冷却すると共に円筒状ドラムにそわ
せ、冷却しながら引張る事により、引取スピード、応力
によりタテ方向の延伸を又、ドラムの寸法によりヨコ方
向の延伸量調整する。The temperature of the resin to the cap is adjusted to 180°C to 240°C, and the temperature of the cap is set 10 to 60°C lower than that. As the base, one that has a slit that is wider than the tip thickness of a coat hanger type or T-die type, or one that is cylindrical and has an annular slit at the tip is used. When using the former type of cap, the resin coming out of the cap is cooled with a roll, the amount of stretching in the vertical direction is adjusted by the take-up speed and stress, and if necessary, the resin is clamped and stretched from the horizontal direction, and then the resin is stretched in the horizontal direction. Adjust the stretching. When using the latter type of die, the foamed resin released from the annular slit is forcibly cooled by jetted gas, and is placed along a cylindrical drum and pulled while cooling, thereby stretching the resin in the vertical direction depending on the drawing speed and stress. Also, the amount of stretching in the horizontal direction is adjusted depending on the dimensions of the drum.
円環状の細隙は、通常0.2〜1.4mmとなされ、円
環状細隙径とドラム径との比、すなわちブローアツプ比
は2.0〜3.0倍に設定される。2.0以下では、押
出方向の縦及び横の加熱収縮後の残存寸法のバランスの
取れた発泡シートを得られ難いし、また3、0以上に延
伸することは無機質を多量に混合しているので困難であ
る。The annular slit is usually 0.2 to 1.4 mm, and the ratio of the annular slit diameter to the drum diameter, that is, the blow-up ratio, is set to 2.0 to 3.0 times. If it is less than 2.0, it will be difficult to obtain a foamed sheet with a well-balanced residual dimension after heat shrinkage in the longitudinal and lateral directions of extrusion, and if it is stretched to more than 3.0, a large amount of inorganic material will be mixed. Therefore, it is difficult.
また、円筒形ドラムは、径の大きい先端部円筒と、径の
やや小さい後端円筒とを連結して使用するのが好ましい
。これにより、冷却されて収縮する円環状樹脂発泡シー
トのドラムへの抵抗を小さくして円滑に引取り、ロール
に巻取ることを簡単に行なうことができる。引取りスペ
ードを上げることが出きるので生産性も良い。また、先
端部ドラムの温度を高くして、押出された円環状樹脂発
泡シートのドラムへの導入を容易にすることも行なわれ
る。Further, it is preferable that the cylindrical drum is used by connecting a leading end cylinder with a large diameter and a rear end cylinder with a slightly smaller diameter. Thereby, the resistance of the annular resin foam sheet, which shrinks upon cooling, against the drum can be reduced so that it can be smoothly taken up and easily wound onto a roll. Productivity is also good because you can increase the takeover spade. Furthermore, the temperature of the tip drum is increased to facilitate the introduction of the extruded annular resin foam sheet into the drum.
この発明において、上記の如く樹脂供給量、発泡剤量、
口金の細隙の大きさ、口金の温度、押出発泡時のブロー
アツプ比、冷却温度、引取りスピード等の押出条件を制
御することにより、密度0.2−1.2 g /c1i
、厚さ0.2−3m+の押出発泡シートであって、19
0℃の雰囲気中で30分間加熱した場合のタテ及びヨコ
方向の収縮率がそれぞれ5〜30%の範囲にあり、且つ
ヨコの残存率とタテの残存率の比が1:0.7〜1:1
.1であ漬ポリオレフィン系樹脂発泡シートが得られる
。密度0.2 g /ad未満では、厚さを厚くしても
曲げ強度が得られず、シートの平滑性が悪くなり鮮明な
印刷ができない。また、1.2 g /1mを超えると
熱成形時に自重によるタレ下がりトラブルが生じる。In this invention, as described above, the amount of resin supplied, the amount of blowing agent,
By controlling the extrusion conditions such as the size of the slit in the die, the temperature of the die, the blow-up ratio during extrusion foaming, the cooling temperature, and the take-up speed, we can achieve a density of 0.2-1.2 g/c1i.
, an extruded foam sheet with a thickness of 0.2-3 m+, 19
The shrinkage rate in the vertical and horizontal directions when heated for 30 minutes in an atmosphere at 0°C is in the range of 5 to 30%, and the ratio of the horizontal survival rate to the vertical survival rate is 1:0.7 to 1. :1
.. A pickled polyolefin resin foam sheet is obtained in step 1. If the density is less than 0.2 g/ad, bending strength cannot be obtained even if the thickness is increased, and the smoothness of the sheet deteriorates, making it impossible to print clearly. Moreover, if it exceeds 1.2 g/1m, troubles will occur due to sagging due to its own weight during thermoforming.
厚さ0.2mm未満では、押出された円環状樹脂発泡シ
ートを円筒ドラムに導入することができないと共に曲げ
強度が不十分で成形用シートとして使用できない、又、
成形前の予熱時に孔が生ずる。If the thickness is less than 0.2 mm, the extruded annular resin foam sheet cannot be introduced into a cylindrical drum, and the bending strength is insufficient so that it cannot be used as a molding sheet.
Pores occur during preheating before molding.
厚さ3.0mmを越えると、押出された円環状樹脂発泡
シートを円筒ドラムに導入して引き取る際にドラムに抵
抗が加わり、引取りが困難である。また、表面が平滑な
発泡シートとならず、印刷性が劣る。When the thickness exceeds 3.0 mm, resistance is added to the drum when the extruded annular resin foam sheet is introduced into the cylindrical drum and taken off, making it difficult to take off. In addition, the foam sheet does not have a smooth surface, resulting in poor printability.
引取りが容易なのは厚さ2.0+mm以下である。A thickness of 2.0+mm or less is easy to take off.
この発泡シートには、厚さ2〜20ミクロンの接着性の
良い熱可塑性樹脂フィルムを積層することにより、熱成
形性、耐油性、その他の物性を改良することができる。By laminating a thermoplastic resin film with a thickness of 2 to 20 microns with good adhesive properties on this foam sheet, thermoformability, oil resistance, and other physical properties can be improved.
また、この発明の190℃の雰囲気中で30分間加熱す
るという意味は、ポリプロピレン系樹脂の結晶融点より
20℃以上の高温の雰囲気中で加熱するものであり、押
出発泡され引き取られたポリプロピレン系樹脂発泡シー
トの結晶構造が全く無くなる温度条件であり、又残留応
力が全く無くなる条件である。In addition, the meaning of heating in an atmosphere of 190°C for 30 minutes in this invention means heating in an atmosphere at a high temperature of 20°C or higher than the crystal melting point of the polypropylene resin, and the polypropylene resin that has been extruded and foamed. This is a temperature condition in which the crystal structure of the foamed sheet is completely eliminated, and also a condition in which residual stress is completely eliminated.
斯くして、この発泡シートを190℃の雰囲気中で30
分間加熱した場合の加熱収縮率が5%より小さいと、加
熱成形時にオーブン中で予熱をするとシートが自重でた
れさがり、成型の位置ずれが起こり、30%より大きい
と深い型の成形ができないばかりでなく、予熱板から外
したときに収縮してしまい、成型板から外れたり、印刷
との成型の位置ずれが起こる。しかし、この加熱収縮率
の好ましい範囲は10〜25%である。また、タテの残
存率の比が0.7未満であると、印刷図形、模様、デザ
インの位置ズレが大きく、図形の予想しない変形が生ず
る。In this way, this foam sheet was heated in an atmosphere of 190°C for 30 minutes.
If the heating shrinkage rate when heated for minutes is less than 5%, the sheet will sag under its own weight when preheated in the oven during hot molding, causing misalignment of the molding, and if it is more than 30%, deep molding will simply not be possible. However, when it is removed from the preheating plate, it shrinks, causing it to come off the molding plate or misaligning the printing and molding. However, the preferable range of this heat shrinkage rate is 10 to 25%. Further, if the ratio of the vertical survival rate is less than 0.7, the positional deviation of the printed figures, patterns, and designs will be large, resulting in unexpected deformation of the figures.
タテの残存率の比が1.1を越えると、円環状ポリプロ
ピレン系樹脂発泡シートをドラムへ導入する際抵抗がか
かりドラムに沿わせること及びシートの引取りが困難で
あり発泡シートの厚みが不均一になる。また、熱成形時
に、両端のクランプの外れが生じ、良い成形品が得られ
ない。If the ratio of the vertical residual ratio exceeds 1.1, there will be resistance when introducing the annular polypropylene resin foam sheet into the drum, making it difficult to align the sheet along the drum and take it off, and the thickness of the foam sheet will be insufficient. It becomes uniform. Furthermore, during thermoforming, the clamps at both ends come off, making it impossible to obtain a good molded product.
印刷のスピードアップ、ゴミの付着を避ける為に樹脂発
泡シートの表面固有抵抗を108〜1012Ωにするた
めに帯電防止剤を樹脂混合物の中に混入してもよいし、
又、発泡シートの表面に薄く塗布してもよい。また、印
刷インキの密着性を向上させる為に発泡シートの表面張
力を向上させるのであるが、表面張力の指数としてぬれ
指数を40dyne/cm以上にすることが好ましく、
ぬれ指数を40dyne/cm以上にするためには界面
活性剤を樹脂混合物のなかへ混入してもよいし、又、発
泡シートの表面に薄く塗布したり、溶剤処理でもよいが
、コロナ放電処理やプラズマ放電処理によって行なうの
が望ましい。An antistatic agent may be mixed into the resin mixture to increase the surface resistivity of the resin foam sheet to 108 to 1012 Ω in order to speed up printing and prevent dust from adhering.
Alternatively, it may be applied thinly to the surface of the foam sheet. In addition, the surface tension of the foam sheet is improved in order to improve the adhesion of printing ink, and it is preferable that the wetting index is 40 dyne/cm or more as an index of surface tension.
In order to achieve a wettability index of 40 dyne/cm or more, a surfactant may be mixed into the resin mixture, or it may be applied thinly to the surface of the foam sheet, or it may be treated with a solvent, but corona discharge treatment or Preferably, this is done by plasma discharge treatment.
この発明の発泡シートは、押出発泡されロール状に巻取
られてそのまま熱成形することもできるが、巻取られた
ロールから加熱ロールに接触させて張力を掛ける加熱処
理によりフラット化し、枚葉にカットして印刷して成形
することもできる。The foamed sheet of this invention can be extruded and foamed, wound up into a roll, and then thermoformed as it is, but it can also be flattened by heating treatment that applies tension by bringing the rolled up roll into contact with a heating roll, and then forming it into sheets. It can also be cut, printed, and shaped.
枚葉にカットした発泡シートは安価なオフセット印刷が
可能であり、更に発泡しているのでインキの密着、吸収
がよく軽量なので積み重ねてもインキ移りが無く、帯電
防止処理をしているので印刷スピードを高速にしてもシ
ートがめくり上がらず、定位置に印刷ができ、次工程で
定位置に成形を施すことができる。Foam sheets cut into sheets can be used for inexpensive offset printing, and since they are foamed, ink adheres well and is absorbed well, and since they are lightweight, there is no ink transfer even when stacked, and the antistatic treatment increases printing speed. Even at high speeds, the sheet does not turn over, printing can be done in a fixed position, and molding can be carried out in a fixed position in the next process.
この発明の発泡シートは、更に、厚み2〜20μ程度の
接着性の良い熱可塑性樹脂フィルムを積層することによ
り熱成形性、耐油性及びその他の物性を改良することが
出来る。The foamed sheet of the present invention can be further improved in thermoformability, oil resistance, and other physical properties by laminating a thermoplastic resin film with good adhesiveness with a thickness of about 2 to 20 μm.
(以下余白)
次に、この発明の実施例及び比較例について詳細に説明
する。(The following is a blank space) Next, Examples and Comparative Examples of the present invention will be described in detail.
実施例1
ポリプロピレン樹脂(住人化学KK、ノーブレンD50
1のベースレジン)70重量部(以下単に部で表わす)
と安定剤(住人化学KK、BHT)0.1部と平均粒径
8μのタルク30部との混合物を押出機によりペレット
を作成した。Example 1 Polypropylene resin (Jumin Chemical KK, Noblen D50
1 base resin) 70 parts by weight (hereinafter simply expressed in parts)
Pellets were prepared using an extruder from a mixture of 0.1 part of a stabilizer (Sumiman Kagaku KK, BHT) and 30 parts of talc having an average particle size of 8 μm.
このペレット100部と帯電防止剤(花王KK、エレク
トロストリッパーTS−2)1部を混合して、シリンダ
ー直径65mmの押出機に供給した。100 parts of these pellets and 1 part of an antistatic agent (Kao KK, Electro Stripper TS-2) were mixed and supplied to an extruder having a cylinder diameter of 65 mm.
そして、直径105mm、細隙0.45mmの円環状細
隙を有する口金を装着して水平方向に押出発泡した。Then, a die having a diameter of 105 mm and an annular slit of 0.45 mm was attached to extrude and foam in the horizontal direction.
押出機シリンダー温度は、200〜230℃に調整し、
シリンダー途中からブタンを約0.5部圧入し、樹脂温
度を200℃に調整して、口金出口の温度を樹脂温度よ
り約10℃低くし、又、口金出口に近傍した20mm以
内に冷却用リングを設け、噴出気体により1.0kg/
a1以下の風圧で内、外面を微風冷却して、1時間25
kgで細隙から円環状発泡樹脂を押出した。The extruder cylinder temperature was adjusted to 200-230°C,
Approximately 0.5 part of butane is injected from the middle of the cylinder, the resin temperature is adjusted to 200°C, and the temperature at the mouthpiece outlet is approximately 10°C lower than the resin temperature. Also, a cooling ring is placed within 20mm near the mouthpiece outlet. 1.0kg/
Cooling the inside and outside with a breeze of wind pressure below A1 for 1 hour 25
kg was extruded from the slit to extrude the annular foamed resin.
この押出された円環状発泡樹脂を入口側直径240II
I11、出口側直径239+sm、長さ50mmの1段
目円筒と入口側直径235mm、出口側直径234++
+m、長さ300mmの2段目円筒とをわずかな隙間を
置いて連結した段差のあるドラムに沿って冷却しながら
引き取る。This extruded annular foam resin has an inlet side diameter of 240 II.
I11, first stage cylinder with exit side diameter 239+sm, length 50mm, inlet side diameter 235mm, exit side diameter 234++
+m and a second stage cylinder with a length of 300 mm are connected to each other with a slight gap between the drums.
この場合、2段目円筒の末端にカッターを取付けて円環
状発泡樹脂を押出方向に切断して発泡シートとした。ブ
ローアツプ比は2.29である。この際、1段目円筒の
冷却温度は、2段目よりも約30℃高くして、引取り抵
抗が減らせて引取り、厚さ0.74mm幅750 mm
密度0.73g/aI?の発泡シートをロール状に捲取
った。In this case, a cutter was attached to the end of the second cylinder to cut the annular foamed resin in the extrusion direction to form a foamed sheet. The blowup ratio is 2.29. At this time, the cooling temperature of the first stage cylinder was set approximately 30°C higher than that of the second stage to reduce the pulling resistance, and the cylinder was pulled out with a thickness of 0.74 mm and a width of 750 mm.
Density 0.73g/aI? The foam sheet was rolled up into a roll.
このシートから押出方向タテ、ヨコ100mmの正方形
シートに切り、この正方形シートを190℃のオーブン
内で30分加熱したところ、加熱後の残存寸法はタテ7
4m(収縮率26%)、ヨコ81mm(収縮率19%)
であり、そのヨコに対するタテの比は0.91であった
。また、表面固有抵抗は10”Ω、ぬれ指数は32dy
ne/ cmであった。This sheet was cut into square sheets measuring 100 mm both vertically and horizontally in the extrusion direction, and when this square sheet was heated in an oven at 190°C for 30 minutes, the remaining dimension after heating was 7 mm vertically.
4m (shrinkage rate 26%), width 81mm (shrinkage rate 19%)
The ratio of vertical to horizontal was 0.91. In addition, the surface resistivity is 10”Ω, and the wetting index is 32dy.
ne/cm.
いったん捲取ったシートを捲緩めながら表裏面をそれぞ
れ150℃に加熱した隣接する二本の加熱ロールの表面
に対してシートをS字形に送りシートの両面を順次接触
、加熱し、次に冷却されている隣接する二本の冷却ロー
ルの表面にシートをS字形に送り、接触させ、張力をか
けながら冷却して引取る。この加熱処理によりロールの
巻き等による変形を解消し、又、発泡シートの厚みの均
一性を良くしたフラットなシートとすると共に、引取る
途中で表裏面にコロナ放電処理を施し、印刷適性を良く
し、両耳及びヨコ方向にカットし、厚さ0.72[11
1幅650膿長さ950 nu密度0.72g/a&の
シートを作成して、成形用の枚葉シートとする。Once the sheet has been rolled up, it is unrolled and the front and back sides are heated to 150°C.The sheet is then sent in an S-shape to the surfaces of two adjacent heating rolls, where both sides of the sheet are successively brought into contact and heated, and then cooled. The sheet is fed in an S-shape onto the surfaces of two adjacent cooling rolls, brought into contact with each other, cooled under tension, and then taken off. This heat treatment eliminates deformation caused by roll winding, etc., and makes the foam sheet a flat sheet with improved thickness uniformity. Corona discharge treatment is applied to the front and back surfaces during collection to improve printing suitability. Then cut both ears and horizontally to a thickness of 0.72 [11
A sheet with a width of 650 mm, a length of 950 mm, and a nu density of 0.72 g/a& is prepared and used as a single sheet for molding.
また、この枚葉シートのフラット性は、1m当り2mm
以下であった。In addition, the flatness of this sheet is 2mm per 1m.
It was below.
また、この枚葉シートから押出方向にタテ、ヨコ100
mmの正方形シートを切取り、190℃のオーブン内で
30分間加熱後の残存寸法が、タテ71mm(収縮率2
9%)、ヨコ83 rm (収縮率17%)で、そのヨ
コに対するタテの比は、0.86であった。ぬれ指数は
46dyne/ cxrrであった。Also, from this sheet, 100 mm vertically and horizontally in the extrusion direction.
After cutting out a square sheet of 1.5 mm in diameter and heating it in an oven at 190°C for 30 minutes, the remaining dimension was 71 mm in length (shrinkage rate 2).
9%), width 83 rm (shrinkage rate 17%), and the length to width ratio was 0.86. Wetting index was 46 dyne/cxrr.
この枚葉シートの成形性については、次のように評価し
た。The moldability of this sheet was evaluated as follows.
ロータリー枚葉成形機を使用し、枚葉シートがら押出方
向に第1図のようにタテ、ヨコ200+amの正方形シ
ートを切取り、このシートを成形型に入れる。シートに
接する熱板による接触加熱面積は、170mm X 1
70n+mであり、成形品のサイズは、150mmX
150nm X深さ20+nmの第2図(a)(b)の
様な容器を熱成形した。Using a rotary single-fed molding machine, cut out a square sheet measuring 200+mm vertically and horizontally from the single-fed sheet in the extrusion direction as shown in FIG. 1, and put this sheet into a mold. The contact heating area by the hot plate in contact with the sheet is 170mm x 1
70n+m, and the size of the molded product is 150mmX
Containers as shown in FIGS. 2(a) and 2(b) measuring 150 nm x 20+ nm deep were thermoformed.
成形時のシート加熱時間を6秒に設定し、加熱温度を1
70℃、180℃、190℃に変えて、タテ又はヨコの
位置ズレ及び伸び、外観を判定した。The sheet heating time during molding was set to 6 seconds, and the heating temperature was set to 1.
The temperature was changed to 70°C, 180°C, and 190°C, and the vertical or horizontal positional deviation, elongation, and appearance were evaluated.
印刷図形の位置ズレの判定として、容器の底部において
成形前にシートの中央に第1図のように十字に直交する
100mm直線を印刷しておき、印刷された線の両端か
らの仮想直線に対する変形量のうち最大の個所を測定し
た。To determine the misalignment of the printed figure, a 100 mm straight line perpendicular to the cross is printed in the center of the sheet at the bottom of the container before molding, as shown in Figure 1, and the deformation of the printed line from both ends relative to the imaginary straight line is determined. The largest part of the amount was measured.
又、容器の側壁の変形量として、成形前に正方形シート
の辺の中央から中心方向50mmの直線に(′A質上、
前記十字の直線の延長線上の直線)印刷しておき、熱成
形後、この印刷された直線の両端からの仮想直線に対す
る変形量のうち最大の個所を測定した。In addition, as the amount of deformation of the side wall of the container, a straight line 50 mm from the center of the side of the square sheet in the center direction ('A due to quality,
A straight line (an extension of the straight line of the cross) was printed, and after thermoforming, the maximum amount of deformation from both ends of the printed straight line with respect to the imaginary straight line was measured.
その変形量が、0 、5mm以内は○、1.0mm以内
はΔ、1 、0mm以上はXと判定した。The amount of deformation was determined to be ○ if it was within 0.5 mm, Δ if it was within 1.0 mm, and X if it was 1.0 mm or more.
又、伸び、外観について、キレツの発生、破れによる成
形不良、部分的極端な薄肉、シワや重なり部分の発生等
で以上のチエツクポイントに、何れも該当しないものは
O1何れか1点だけ該当するものはΔ、何れも該当する
ものは×と判定した。In addition, regarding elongation and appearance, if none of the above check points apply due to occurrence of cracks, defective molding due to tearing, extremely thin parts, occurrence of wrinkles or overlapping parts, etc., only one of the above points applies. Those that met were rated as Δ, and those that met were rated as ×.
これらの判定結果を第3表に記載した。また、同様に他
の実施例及び比較例についても第3表にその結果を記載
した。These determination results are listed in Table 3. Similarly, the results of other Examples and Comparative Examples are also listed in Table 3.
実施例2
実施例1の方法において、帯電防止剤を取り除いた以外
は、全く同様に行なった。Example 2 The same procedure as in Example 1 was repeated except that the antistatic agent was removed.
ロール状に捲取られた発泡シートは、厚さ0.73m、
幅750℃密度0.72 g /cn?で表面固有抵抗
は1017Ωであった。The foam sheet rolled into a roll has a thickness of 0.73 m.
Width 750℃ Density 0.72 g/cn? The surface resistivity was 1017Ω.
又、同様の加熱後の残存寸法は、タテ79oa(収縮率
21%)、ヨコ84m(収縮率16%)で、その比は0
.94であった。In addition, the remaining dimensions after similar heating are 79 oa vertically (21% shrinkage) and 84 m horizontally (16% shrinkage), and the ratio is 0.
.. It was 94.
同様の加熱処理により、フラット化とコロナ放電処理及
びカットし、厚さ0.72m++幅650m長さ950
nm密度0.74g/ai?の枚葉シートとした。By the same heat treatment, it is flattened, corona discharge treated and cut to a thickness of 0.72m++, width of 650m, length of 950mm.
nm density 0.74g/ai? It was made into a single sheet.
また、二〇枚葉シートのフラット性は、1111当り2
+am以下であった。In addition, the flatness of 20 sheets is 2 per 1111
+am or less.
加熱後の残存寸法は、タテ74in(収縮率26%)、
ヨコ85mm(収縮率15%)で、その比は、0.87
であり、ぬれ指数は44dyne/ amであった。The remaining dimensions after heating are 74 inches vertically (shrinkage rate 26%),
Width 85mm (shrinkage rate 15%), the ratio is 0.87
The wetting index was 44 dyne/am.
実施例3
樹脂として、ポリプロピレン樹脂(住人化学KK、ノー
ブレンAD571)50部と高密度ポリエチレン樹脂(
三菱油化KK、ユカロンHD、 JX−10)20部と
、炭カル(竹原化学KK、サンライト#700、平均粒
径4.5μ)30部を混合して押出機でペレットを作成
した。Example 3 As resins, 50 parts of polypropylene resin (Jumin Chemical KK, Noblen AD571) and high density polyethylene resin (
20 parts of Mitsubishi Yuka KK, Yucalon HD, JX-10) and 30 parts of Charcoal (Takehara Kagaku KK, Sunlight #700, average particle size 4.5 μm) were mixed to form pellets using an extruder.
他は、実施例1と同じ方法でシートを得た。A sheet was obtained in the same manner as in Example 1 in other respects.
捲取られた発泡シートは、厚さ0 、80mm幅750
I密度0 、70g/ crjで、同様の加熱後の残存
寸法は、タテ76I(収縮率24%)、ヨコ88mm(
収縮率12%)で、その比は、0.86であった。The rolled up foam sheet has a thickness of 0, a width of 80 mm and a width of 750 mm.
With an I density of 0 and 70 g/crj, the remaining dimensions after similar heating are 76 I (vertical) (shrinkage rate 24%) and 88 mm (horizontal) (
The shrinkage rate was 12%), and the ratio was 0.86.
表面固有抵抗は1011Ω、ぬれ指数は32dyne/
amであった。Surface resistivity is 1011Ω, wetting index is 32dyne/
It was am.
実施例4
実施例1と同様にして行なったが、樹脂としては、ポリ
プロピレン樹脂とタルクの比率を80対20部として、
発泡剤としては、重曹とクエン酸の混合物(大日精化に
に、ダイブロー#2)を1部混合した。Example 4 The same procedure as in Example 1 was carried out, except that the ratio of polypropylene resin to talc was 80:20 parts.
As a foaming agent, one part of a mixture of baking soda and citric acid (Dainichiseika Chemical Co., Ltd., Daiblow #2) was mixed.
又、帯電防止剤は押出機への配合を止め、押出したシー
トへ塗布した。Further, the antistatic agent was stopped from being added to the extruder and was applied to the extruded sheet.
捲き取られた発泡シートは、厚さ1.10ma+幅75
0I密度0.50g/aJで、同様の加熱後の残存寸法
は、タテ75m(収縮率25%)、ヨコ90am(収縮
率10%)で、その比は、0.83であり、表面固有抵
抗は1016Ωであった。The rolled up foam sheet has a thickness of 1.10ma and a width of 75mm.
At an 0I density of 0.50 g/aJ, the remaining dimensions after similar heating are 75 m vertically (25% shrinkage rate) and 90 am horizontally (10% shrinkage rate), and the ratio is 0.83, and the surface resistivity is was 1016Ω.
一旦捲取ったシートを捲緩めながら、表裏面に帯電防止
剤水溶液(ヘキストKK、ホスタスタットus−1)を
薄く塗布し、実施例1と同様の方法で、加熱ロールで加
熱処理と乾燥を行なってフラット化を行なった。While unwinding the sheet once rolled up, an aqueous antistatic agent solution (Hoechst KK, Hostastat US-1) was applied thinly to the front and back surfaces, and heat treatment and drying were performed using a heating roll in the same manner as in Example 1. flattened.
又、引取る途中で、表裏面にコロナ放電処理を施し、印
刷適性を良くして、両耳及びヨコ方向にカットし、厚さ
1.Oai幅650I長さ950℃密度0.52g/a
d、フラット性は、1m当り21all以下の枚葉シー
トとした。In addition, during collection, corona discharge treatment is applied to the front and back surfaces to improve printing suitability, and the paper is cut on both sides and in the horizontal direction to a thickness of 1. Oai width 650I length 950℃ density 0.52g/a
d. The flatness of the sheet was 21all or less per 1m.
この枚葉シートを同様に加熱後の残存寸法は、タテ73
mn1(収縮率27%)、ヨコ91m(収縮率9%)で
、その比は、0.80であり、表面固有抵抗は1012
Ω、ぬれ指数は44dyne/ amであった。The remaining dimension after heating this sheet in the same way is 73 mm vertically.
mn1 (shrinkage rate 27%), width 91m (shrinkage rate 9%), the ratio is 0.80, and the surface specific resistance is 1012
Ω, wetting index was 44 dyne/am.
実施例5
ポリプロピレン樹脂とタルクの比率を60対40部とし
た以外は実施例4と同様に行なった。Example 5 The same procedure as Example 4 was carried out except that the ratio of polypropylene resin to talc was 60:40 parts.
捲き取られた発泡シートは、厚さ1 、10+am幅7
50m密度0.61g/adで、同様に加熱後の残存寸
法は、タテ741111(収縮率26%)、ヨコ78m
(収縮率22幻で、その比は、0.95であり、表面固
有抵抗は1016Ωであった。The rolled up foam sheet has a thickness of 1 mm and a width of 10 + 7 am.
50m density is 0.61g/ad, and the remaining dimensions after heating are 741111 (vertical) (shrinkage rate 26%) and 78m (horizontal).
(The shrinkage rate was 22, the ratio was 0.95, and the surface resistivity was 1016Ω.
更に、実施例4と同様に、帯電防止剤の塗布及び加熱ロ
ールで加熱処理、コロナ放電処理、及びカットを行ない
、厚さ1.01幅650ffl長さ950 mm密度0
.65g/c+J、フラット性は、2思−以下の枚葉シ
ートが得られた。Furthermore, in the same manner as in Example 4, an antistatic agent was applied, heat treatment was performed using a heating roll, corona discharge treatment, and cutting was performed to obtain a product with a thickness of 1.01, a width of 650 ffl, a length of 950 mm, and a density of 0.
.. A sheet with a flatness of 65 g/c+J and a flatness of 2 mm or less was obtained.
この枚葉シートを同様に加熱後の残存寸法は、タテ70
m(収縮率30%)、ヨコ80m(収縮率20%)で、
その比は、0.87であり、表面固有抵抗は1010Ω
、ぬれ指数は44dyne/ csであった。The remaining dimension after heating this sheet in the same way is 70 mm vertically.
m (shrinkage rate 30%), width 80m (shrinkage rate 20%),
The ratio is 0.87 and the surface resistivity is 1010Ω
, the wetting index was 44 dyne/cs.
実施例6
ポリプロピレン樹脂(住人化学KK、ノーブレンD50
1のベースレジン)70部と安定剤(住人化学KK、B
HT)0.1部と平均粒径8μのタルク30部との混合
物を押出機によりペレットを作成した。Example 6 Polypropylene resin (Jumin Chemical KK, Noblen D50
1 base resin) 70 parts and stabilizer (Jumin Chemical KK, B
HT) and 30 parts of talc having an average particle size of 8 μm were made into pellets using an extruder.
このペレット100部をシリンダー直径90mmの押出
機に供給した。そして、直径180mm、細隙0.50
mmの円環状細隙を有する口金を装着して下向きに押出
発泡した。100 parts of the pellets were fed into an extruder having a cylinder diameter of 90 mm. And diameter 180mm, slit 0.50
A nozzle having an annular gap of mm was attached and foam was extruded downward.
押出機シリンダー温度は、200〜240℃に調整し、
シリンダー途中からブタンを約0.5部圧入し、樹脂温
度を220℃に調整して、口金出口の温度を樹脂温度よ
り約10℃低くし、又、口金出口に近接した20mm以
内に冷却リングを設け、噴出気体により1.0kg/a
J以下の風圧で内、外面を微風冷却して、・1時間80
kgで細隙から円環状発泡樹脂を押出した。The extruder cylinder temperature was adjusted to 200-240°C,
About 0.5 part of butane is pressurized from the middle of the cylinder, the resin temperature is adjusted to 220°C, the temperature at the mouthpiece outlet is about 10°C lower than the resin temperature, and a cooling ring is installed within 20mm close to the mouthpiece outlet. 1.0kg/a by blowing gas
By cooling the inner and outer surfaces with a breeze of wind pressure below J, 80°C for 1 hour.
kg was extruded from the slit to extrude the annular foamed resin.
この押出された円環状発泡樹脂を入口側直径455mm
、出口側直径454mm、長さ70+usの1段目円筒
と入口側直径450mm、出口側直径448mm、長さ
4301Ifflの2段目円筒とをわずかな隙間を置い
て連結した段差のあるドラムに沿って冷却しながら引き
取る。この場合のブローアツプは、2.53である。This extruded annular foam resin has a diameter of 455 mm on the inlet side.
, along a stepped drum in which a first stage cylinder with an exit side diameter of 454 mm and a length of 70+us and a second stage cylinder with an inlet side diameter of 450 mm, an exit side diameter of 448 mm and a length of 4301 Iffl are connected with a slight gap. Remove while cooling. The blowup in this case is 2.53.
そして、2段目円筒の末端に2個のカッターを取付けて
円環状発泡樹脂を押出方向に2等分に切断して2個の発
泡シートとした。タルク等の無機質微粉末の混合する量
が多くなると、冷却された円筒ドラムに沿わせて導入す
る作業が困難になるが、この実施例のように下向に押し
出すと円筒ドラムの導入する作業が比較的容易になる。Then, two cutters were attached to the ends of the second-stage cylinder to cut the annular foamed resin into two equal parts in the extrusion direction to obtain two foamed sheets. If the amount of inorganic fine powder such as talc to be mixed increases, it becomes difficult to introduce it along the cooled cylindrical drum, but if it is pushed downward as in this example, the work of introducing the cylindrical drum becomes easier. It becomes relatively easy.
又、1段目円筒の冷却温度は、2段目よりも約30℃高
くして、引取り抵抗が減らせて引取り発泡シートを2本
のロール状に捲取った。In addition, the cooling temperature of the first stage cylinder was set to be about 30° C. higher than that of the second stage to reduce the pulling resistance, and the foamed sheet was rolled up into two rolls.
この捲取られた発泡シートは、厚さ0.73部m、幅7
00nm密度0.81g/aJで表面固有抵抗は10”
Ω、ぬれ指数は32dyne/amあった。同様に加熱
後の残存寸法は、タテ85m(収縮率15%)、ヨコ8
7m(収縮率13%)で、その比は、0.98であった
。This rolled up foam sheet has a thickness of 0.73 parts m and a width of 7 m.
00nm density 0.81g/aJ and surface resistivity 10"
Ω, and the wetting index was 32 dyne/am. Similarly, the remaining dimensions after heating are 85 m vertically (shrinkage rate 15%) and 8 m horizontally.
At 7 m (shrinkage rate 13%), the ratio was 0.98.
−旦捲取ったシートを捲緩めながら、表裏面をそれぞれ
150℃に加熱されたロールに接触させ、張力をかけな
がら、冷却して引取り、加熱処理によりフラットなシー
トにした。引取る途中で表裏面にコロナ放電を施し、帯
電防止剤水溶液(日本純薬KK、 5AT−5)を微細
な霧状にしてシートに吹付は薄く塗膜を形成させてから
約80℃の温度で乾燥を施し、両耳及びヨコ方向にカッ
トし、厚さ0.72m幅650 m長さ950I111
密度0.83g/ad、シートのフラット性は、1m当
り2mm以下の枚葉シートとした。- While loosening the rolled sheet, the front and back surfaces were brought into contact with rolls heated to 150°C, and while applying tension, the sheet was cooled and taken off, and a flat sheet was formed by heat treatment. During collection, corona discharge is applied to the front and back surfaces, and a fine mist of antistatic agent aqueous solution (Nippon Pure Chemical Industries, Ltd., 5AT-5) is sprayed onto the sheet to form a thin film, and then the sheet is heated to a temperature of approximately 80°C. Dry it and cut it in both ears and horizontal direction, thickness 0.72m width 650m length 950I111
The density of the sheet was 0.83 g/ad, and the flatness of the sheet was 2 mm or less per 1 m.
二〇枚葉シートから同様に加熱後の残存寸法は。The remaining dimensions after heating in the same way from 20 sheets.
タテ84m(収縮率16%)、ヨコ87m(収縮率13
%)で、その比は、0.97であり、表面固有抵抗は1
010Ω、ぬれ指数は48dyne/ rxであった。Vertical 84m (shrinkage rate 16%), width 87m (shrinkage rate 13%)
%), the ratio is 0.97, and the surface resistivity is 1
010 Ω, and the wetting index was 48 dyne/rx.
実施例7
直径180mm、細隙0.35mmの円環状細隙を有す
る口金を装着する以外は実施例6と同じ方法で行なった
・
この捲取られた発泡シートは、厚さ0.48m、幅70
0部密度0.43 g /ciで、表面固有抵抗は10
”Ω、ぬれ指数は32dyne/ alあった。同様に
加熱後の残存寸法は、タテ80m5(収縮率20%)、
ヨコ88醜(収縮率12%)で、その比は、0.91で
あった。Example 7 The same method as in Example 6 was carried out except that a cap having a diameter of 180 mm and an annular slit of 0.35 mm was attached. This rolled-up foam sheet had a thickness of 0.48 m and a width of 0.48 m. 70
0 part density is 0.43 g/ci, surface resistivity is 10
"Ω, wetting index was 32 dyne/al. Similarly, the remaining dimensions after heating were 80 m5 (vertical) (20% shrinkage),
The width was 88 ugly (shrinkage rate 12%), and the ratio was 0.91.
−旦捲取ったシートを実施例6と同様に加熱処理、コロ
ナ放電処理、帯電防止剤水溶液(日本純薬KK、 5A
T−5)を施し、両耳及びヨコ方向にカットし、厚さ0
.46mm 幅650m長さ950部密度0.46に/
−シートのフラット性は、1mm以下の枚葉シートとし
た。- The rolled sheet was subjected to heat treatment, corona discharge treatment, and antistatic agent aqueous solution (Nippon Pure Chemical Industries, Ltd., 5A) in the same manner as in Example 6.
T-5) and cut in both ears and horizontal direction, thickness 0
.. 46mm Width 650m Length 950 parts Density 0.46 /
- The flatness of the sheet was 1 mm or less.
この枚葉シートから同様に加熱後の残存寸法は。The remaining dimensions of this sheet after heating are as follows.
タテ78m(収縮率22%)、ヨコ84mn+(収縮率
16%)で、その比は、0.93であり、表面固有抵抗
は1o10Ω、ぬれ指数は49dyne/ csaであ
った。The length was 78 m (shrinkage rate 22%) and the width was 84 m+ (shrinkage rate 16%), the ratio was 0.93, the surface resistivity was 1010Ω, and the wettability index was 49dyne/csa.
実施例8
ポリプロピレン樹脂(住友化学にK、ノーブレンD50
1のベースレジン)70部と安定剤(住友化学にK、B
IT)0.1部と平均粒径8μのタルク3o部との混合
物を押出機によりペレットを作成した。Example 8 Polypropylene resin (K to Sumitomo Chemical, Noblen D50
70 parts of base resin (1) and stabilizer (K, B to Sumitomo Chemical)
A mixture of 0.1 part of IT) and 30 parts of talc having an average particle size of 8 microns was made into pellets using an extruder.
このペレット100部を発泡体原料とした6発泡体原料
を直径9011!11の押出機に供給した。6 Foam raw materials using 100 parts of these pellets as foam raw materials were supplied to an extruder having a diameter of 9011!11.
他方、ポリプロピレン樹脂(住友化学KKノーブレンF
S2011D)をフィルム原料とした。On the other hand, polypropylene resin (Sumitomo Chemical KK Noblen F
S2011D) was used as a film raw material.
フィルム原料を直径50m111の押出機と直径45m
mの押出機にも供給し、前記直径90m+iの押出機に
合流せしめて、前記発泡体の両面にフィルム層を設ける
ように共押出して積層発泡シートを製造した。The film raw material is transferred to an extruder with a diameter of 50m111 and an extruder with a diameter of 45m.
The mixture was also supplied to an extruder with a diameter of 90 m+i, and coextruded to form a film layer on both sides of the foam to produce a laminated foam sheet.
この際、押出機の先端に、直径180mm、細隙0 、
50mmの円環状細隙を有する口金を装置して下向きに
押出発泡した。At this time, at the tip of the extruder, a diameter of 180 mm, a slit of 0,
A nozzle with a 50 mm annular gap was installed and foam was extruded downward.
以下、実施例6と同様に操作して、積層発泡シートの物
性及びその成形性は第4表の通りであった。Thereafter, the same operations as in Example 6 were carried out, and the physical properties and moldability of the laminated foam sheet were as shown in Table 4.
比較例1
実施例1において、押出された円環状発泡樹脂を、直径
200+++o、長さ300mmの円筒からなるドラム
に沿わせて冷却しながら引き取った。これは、ブローア
ツプ比は、1.90である。Comparative Example 1 In Example 1, the extruded annular foamed resin was taken along a drum consisting of a cylinder with a diameter of 200+++o and a length of 300 mm while being cooled. This has a blowup ratio of 1.90.
この捲取られた発泡シートは、厚さ0.73mm、幅6
20mm、密度0.71g/at?であり、同様に加熱
後の残存寸m I!、9 テ52ramC収縮率48%
)、E :]882m+m収縮率18%)であり、その
比は、0.63であった。表面固有抵抗は、1o11Ω
であったが、ぬれ指数は3zdyne/cm Lかなが
った。This rolled up foam sheet has a thickness of 0.73 mm and a width of 6
20mm, density 0.71g/at? Similarly, the remaining size after heating m I! , 9 Te52ramC contraction rate 48%
), E:]882m+m shrinkage rate 18%), and the ratio was 0.63. Surface resistivity is 1o11Ω
However, the wettability index was higher than 3zdyne/cm L.
比較例2
実施例6において、押出された円環状発泡樹脂を、入口
側直径340mm、出口側直径339mm、長さ7◇I
IImの1段目円筒と、入口側直径335mm、出口側
直径333a+m、 Qさ430m+sの2段目円筒と
をわずかな隙間を置いて連結した段差のあるドラムに沿
って冷却しながら引取る。このブローアツプ比は、1.
89である。Comparative Example 2 In Example 6, the extruded annular foamed resin had a diameter of 340 mm on the inlet side, a diameter of 339 mm on the outlet side, and a length of 7◇I.
A first-stage cylinder of IIm and a second-stage cylinder with an inlet side diameter of 335 mm, an outlet side diameter of 333 a+m, and a Q length of 430 m+s are connected with a slight gap, and are taken while cooling along a drum with a step. This blow-up ratio is 1.
It is 89.
そして、2段目円筒の末端に1個のカッターを取付けて
、円環状発泡樹脂を押出方向に切断して発泡シートとし
た。Then, a cutter was attached to the end of the second stage cylinder, and the annular foamed resin was cut in the extrusion direction to form a foamed sheet.
又、実施例6と同様に、発泡シートをロール状に捲取っ
た。Further, in the same manner as in Example 6, the foam sheet was rolled up into a roll.
この捲取られた発泡シートは、厚さ0.70mm、幅1
050mm、密度0.77g/cdで、表面固有抵抗は
、1016Ω、ぬれ指数は32dyne/amであった
。又、同様に加熱後の残存寸法は、タテ52mm(収縮
率48%)、ヨコ86mm(収縮率14%)であり、そ
の比は、0.60であった・
このように成形性について、各実施例では容器の底部及
び側壁において、殆どが0.5mm以内の位置ズレに抑
えられているが、一方、比較例では1 、 On+m以
上の位置ズレが生じている。This rolled up foam sheet has a thickness of 0.70 mm and a width of 1
050 mm, density 0.77 g/cd, surface resistivity was 1016 Ω, and wetting index was 32 dyne/am. Similarly, the remaining dimensions after heating were 52 mm vertically (48% shrinkage rate) and 86 mm horizontally (14% shrinkage rate), and the ratio was 0.60. In this way, regarding moldability, each In the examples, most of the positional deviations were suppressed to within 0.5 mm at the bottom and side walls of the containers, whereas in the comparative examples, positional deviations of 1.On+m or more occurred.
また、図3 (a) (b) (c)の成形品は、この
発明の発泡シートで熱成形された菓子等の収容に使用さ
れる人形形状の容器であり、中央にヒンジ部を介して両
側に収容部がある。そして、発泡シートの表面に印刷さ
れた人形図形と凹凸模様がほぼ一致している。The molded products shown in FIGS. 3(a), 3(b), and 3(c) are doll-shaped containers used for storing confectionery etc. thermoformed with the foam sheet of the present invention, There are storage compartments on both sides. The doll figure printed on the surface of the foam sheet and the uneven pattern almost match.
また、図4 (a) (b)の成形品は、同様に熱成形
された蓋付包装用容器であり、容器本体の側壁は二重に
折返された深絞り成形が出来ることを示している。The molded products shown in Figures 4 (a) and 4 (b) are similarly thermoformed packaging containers with lids, and the side walls of the container body are double folded, indicating that deep drawing can be performed. .
(以下余白)
(発明の効果)
以上、詳細に述べたとおり、この発明のポリプロピレン
系樹脂発泡シートは、熱成形性の点で特有の効果を有す
る。又、この製造方法は円筒ドラムを改良することによ
り引取りスピードの向上を計り、生産性を改善したもの
である。(The following is a blank space) (Effects of the Invention) As described above in detail, the polypropylene resin foam sheet of the present invention has a unique effect in terms of thermoformability. In addition, this manufacturing method improves productivity by improving the take-up speed by improving the cylindrical drum.
斯くして、この発泡シートに所定図形を印刷して熱成形
すれば、印刷図形模様の位置ズレの少ない美麗な成形品
及び複雑な立体構造のある精巧な成形品が製造できる。By printing a predetermined figure on this foam sheet and thermoforming it, it is possible to produce a beautiful molded product with little misalignment of the printed graphic pattern and a sophisticated molded product with a complex three-dimensional structure.
従って、これらの成形品は1食品容器、包装容器等の容
器または立体模様のある表示パネルとして好適なもので
ある。Therefore, these molded products are suitable as containers such as food containers and packaging containers, or display panels with three-dimensional patterns.
第1図は、この発明の実施例及び比較例のポリプロピレ
ン系樹脂発泡シートの平面図、第2図(a)は第1図の
発泡シートを熱成形した容器の平面図、第2図(b)は
第2図(a)をトリミングした容器の正面断面図、第3
図(a) (b) (c)は、この発明の発泡シートか
ら成形した人形形状の容器で、それぞれその側面図、展
開された平面図、側面断面図、第4図(a) (b)は
、この発明発泡シートから成形した蓋付包装容器でそれ
ぞれその切欠斜視図、側面断面図ある。
出願人 積水化成品工業株式会社FIG. 1 is a plan view of polypropylene resin foam sheets of Examples and Comparative Examples of the present invention, FIG. 2(a) is a plan view of a container thermoformed from the foam sheet of FIG. 1, and FIG. ) is a front cross-sectional view of the container after FIG. 2(a) has been cropped;
Figures (a), (b), and (c) show a doll-shaped container molded from the foamed sheet of the present invention, and its side view, unfolded plan view, side sectional view, and Figure 4 (a) (b) respectively. The following are a cutaway perspective view and a side sectional view of a packaging container with a lid formed from the foamed sheet of the present invention, respectively. Applicant Sekisui Plastics Co., Ltd.
Claims (1)
重量%均質に混合された、密度0.2〜1.2g/m^
3、厚さ0.2〜3mmの押出発泡シートであって、1
90℃の雰囲気中で30分間加熱した場合のタテ及びヨ
コ方向の収縮率がそれぞれ5〜30%の範囲にあり、且
つヨコの残存率とタテの残存率の比が1:0.7〜1:
1.1であることを特徴とする熱成形性の良いポリプロ
ピレン系樹脂発泡シート。 2、熱可塑性樹脂フィルムが積層されていることを特徴
とする請求項第1項記載のポリプロピレン系樹脂発泡シ
ート。 3、ポリプロピレン系樹脂に無機質微粉末と発泡剤を均
質に混合せしめて押出発泡せしめる方法において、該樹
脂に対して10〜50重量%の無機質微粉末を混合せし
め、押出機先端に装着した円環状細隙を有する口金から
押出発泡させ、該円環状ポリプロピレン系樹脂発泡シー
トを上記円環状細隙の径の2.0〜3.0倍の径を持つ
円筒形ドラムに沿わせて冷却しながら引き取ることを特
徴とする請求項第1項記載の熱成形性の良いポリプロピ
レン系樹脂発泡シートの製造方法。 4、円筒形ドラム経過の円環状ポリプロピレン系樹脂発
泡シートを押出方向に切断し、この発泡シートの表面を
加熱されたロールに接触させて張力を加えて引取り、ヨ
コ方向に切断することを特徴とする請求項第3項記載の
熱成形性の良いポリプロピレン系樹脂発泡シート製造方
法。[Claims] 1. 10 to 50% inorganic fine powder in polypropylene resin
Weight% homogeneously mixed, density 0.2-1.2g/m^
3. An extruded foam sheet with a thickness of 0.2 to 3 mm, 1
The shrinkage rate in the vertical and horizontal directions when heated for 30 minutes in an atmosphere of 90°C is in the range of 5 to 30%, and the ratio of the horizontal survival rate to the vertical survival rate is 1:0.7 to 1. :
A polypropylene resin foam sheet with good thermoformability, characterized by a temperature of 1.1. 2. The polypropylene resin foam sheet according to claim 1, characterized in that a thermoplastic resin film is laminated thereon. 3. In a method of homogeneously mixing inorganic fine powder and a foaming agent with polypropylene resin and extrusion foaming, 10 to 50% by weight of inorganic fine powder is mixed with the resin, and a circular ring attached to the tip of an extruder is used. The foam is extruded through a die having a slit, and the annular polypropylene resin foam sheet is taken along a cylindrical drum having a diameter 2.0 to 3.0 times the diameter of the annular slit while being cooled. 2. The method for producing a polypropylene resin foam sheet with good thermoformability according to claim 1. 4. A circular polypropylene resin foam sheet shaped like a cylindrical drum is cut in the extrusion direction, the surface of the foam sheet is brought into contact with a heated roll, tension is applied, and the sheet is taken up and cut in the horizontal direction. The method for producing a polypropylene resin foam sheet with good thermoformability according to claim 3.