JPH0133657B2 - - Google Patents

Info

Publication number
JPH0133657B2
JPH0133657B2 JP58075184A JP7518483A JPH0133657B2 JP H0133657 B2 JPH0133657 B2 JP H0133657B2 JP 58075184 A JP58075184 A JP 58075184A JP 7518483 A JP7518483 A JP 7518483A JP H0133657 B2 JPH0133657 B2 JP H0133657B2
Authority
JP
Japan
Prior art keywords
fibers
piston
inorganic fiber
ring groove
inorganic
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
JP58075184A
Other languages
Japanese (ja)
Other versions
JPS59201953A (en
Inventor
Tsugio Iino
Wataru Shioda
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Mahle Engine Components Japan Corp
Original Assignee
Izumi Automotive Industry Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Izumi Automotive Industry Co Ltd filed Critical Izumi Automotive Industry Co Ltd
Priority to JP7518483A priority Critical patent/JPS59201953A/en
Publication of JPS59201953A publication Critical patent/JPS59201953A/en
Publication of JPH0133657B2 publication Critical patent/JPH0133657B2/ja
Granted legal-status Critical Current

Description

【発明の詳細な説明】 本発明は内燃機関用のピストンに係り、とくに
金属によつて鋳造されるとともに、その外周面お
よび頂部にそれぞれリング溝および凹部から成る
燃焼室を備えるピストンに関する。
DETAILED DESCRIPTION OF THE INVENTION The present invention relates to a piston for an internal combustion engine, and more particularly to a piston that is cast from metal and has a combustion chamber formed of a ring groove and a recess on its outer peripheral surface and top, respectively.

内燃機関の性能の向上に伴なつて、内燃機関を
構成する各種の部品にもそれぞれ大きな負荷が加
わるようになつており、とくに内燃機関を構成す
る主要部品であるピストンにおいては、高い機械
的な負荷と熱的な負荷が加えられるようになつて
きている。従つて高性能の内燃機関に取付けられ
るピストンは、このような負荷に耐えるものでな
ければならない。そしてとくにピストン1の場合
には、第1図に示すようにそのトツプリング溝2
が高い耐摩耗性を要求されている。また直接噴射
型内燃機関に用いられるピストンは、その頂面に
凹部から成る燃焼室3が設けられることになり、
この燃焼室3の開口縁部が高い熱的な負荷を受け
て亀裂4を生じ易くなる。
As the performance of internal combustion engines improves, large loads are being applied to the various parts that make up the engine.In particular, the pistons, which are the main parts that make up the internal combustion engine, are subject to high mechanical stress. Loads and thermal loads are being added. Therefore, pistons installed in high-performance internal combustion engines must be able to withstand such loads. In particular, in the case of the piston 1, its top ring groove 2 is
is required to have high wear resistance. In addition, the piston used in a direct injection internal combustion engine is provided with a combustion chamber 3 consisting of a recess on its top surface.
The opening edge of the combustion chamber 3 is subjected to a high thermal load, and cracks 4 are likely to occur.

このような機械的あるいは熱的な負荷を受ける
トツプリング溝や燃焼室の開口縁部の強化のため
に、各種の対策がなされている。例えばトツプリ
ング溝2の補強の例としては、異種金属のリング
を装着する試みがなされている。また燃焼室3の
開口縁部の熱亀裂の対策としては、この部分に鋼
材をインサートし、あるいはセラミツクから成る
別の部材を結合し、あるいはまた硬質陽極酸化皮
膜を生成させる等の対策がなされている。
Various measures have been taken to strengthen the top spring groove and the opening edge of the combustion chamber, which are subject to such mechanical or thermal loads. For example, as an example of reinforcing the top ring groove 2, attempts have been made to attach a ring made of a different metal. In addition, measures have been taken to prevent thermal cracks at the opening edge of the combustion chamber 3, such as inserting a steel material into this area, bonding another member made of ceramic, or forming a hard anodic oxide film. There is.

さらに別の対策としては、近年とくに進歩が著
しい無機繊維による補強があげられる。一般に無
機繊維は、ガラス繊維、金属繊維、セラミツク繊
維の3種類があげられるが、内燃機関用のピスト
ンに利用されるものは、その製造性および製造後
の特性等を考慮して、セラミツク繊維が考えられ
ている。
Another countermeasure is reinforcement using inorganic fibers, which has been particularly advanced in recent years. In general, there are three types of inorganic fibers: glass fibers, metal fibers, and ceramic fibers, but ceramic fibers are used for pistons for internal combustion engines, considering their manufacturability and post-manufacturing properties. It is considered.

セラミツク繊維は大別すると、連続繊維、非結
晶の短繊維、結晶短繊維、およびウイスカの4種
類に分けられる。第1の連続繊維は、有機材繊維
を製造し、これを酸化あるいは炭化等の化学処理
によつてセラミツク化するものであつて、一般に
直径は太く、10μ程度のものが多い。つぎに第2
の非結晶の短繊維は、セラミツク組成の溶融体を
ブローニングあるいはスピニング等の方法によつ
て繊維化するものであつて、その直径は2〜5μ、
長さは最大250mm程度である。そしてこの繊維は
セラミツクの非晶質であつて、これを熱処理する
ことにより結晶とすることができる。またこの繊
維の特徴は、その製造の際にシヨツトと呼ばれる
粒状物が混入することである。このシヨツトは切
断、水中解縺、遠心分離、ふるい分け等の工程を
経てある程度除去することができる。つぎに第3
の結晶短繊維は、上記第2の短繊維と類似の方法
で製造され、ほぼ50mm以下の短繊維から構成され
るために、その直径も3〜5μ程度になり、直径
が細くなるという特徴を有する。そして熱処理を
行なうことによつて結晶化されている。つぎに第
4のウイスカはひげ状の単結晶から構成され、そ
の直径は1μ以下であつて、長さも0.2mm以下のも
のが多い。
Ceramic fibers can be roughly divided into four types: continuous fibers, amorphous short fibers, crystalline short fibers, and whiskers. The first continuous fibers are produced by manufacturing organic fibers and turning them into ceramics by chemical treatment such as oxidation or carbonization, and generally have a large diameter of about 10 μm. Then the second
The amorphous short fibers are obtained by turning a melt of ceramic composition into fibers by methods such as browning or spinning, and have a diameter of 2 to 5 μm.
The maximum length is about 250mm. This fiber is an amorphous ceramic, and can be made crystalline by heat-treating it. Another feature of this fiber is that particulate matter called shot is mixed into it during its manufacture. This shot can be removed to some extent through processes such as cutting, underwater disintegration, centrifugation, and sieving. Then the third
The short crystalline fibers are produced in a similar manner to the second short fiber, and are composed of short fibers of approximately 50 mm or less, so their diameter is approximately 3 to 5 μm, making them thinner in diameter. have It is then crystallized by heat treatment. Next, the fourth whisker is composed of whisker-like single crystals, and its diameter is 1 μ or less, and the length is often 0.2 mm or less.

ところでアルミニウム合金等の金属によつて鋳
造されるピストンを繊維で複合する目的は、上述
の如く耐摩耗性を向上させ、あるいは応力破壊に
耐えるようにするためである。さらに金属によつ
て鋳造されたピストンは、その後に精密な機械加
工を行なうために、この機械加工に順応するもの
でなければならない。またピストンには疲労等の
比較的弱い応力が加えられるために、これらの応
力についても考慮しなければならない。そしてこ
れらの目的を達するための特性を与える因子とし
ては、複合強化される繊維の種類や太さおよび長
さ、複合される繊維に混在されるシヨツト等があ
げられる。
By the way, the purpose of composite pistons cast from metal such as aluminum alloy with fibers is to improve wear resistance or to resist stress fracture as described above. Additionally, the piston cast from metal must be compatible with subsequent precision machining. Furthermore, since relatively weak stresses such as fatigue are applied to the piston, these stresses must also be taken into consideration. Factors that give properties to achieve these objectives include the type, thickness, and length of the fibers to be composite reinforced, shots mixed in the fibers to be composited, and the like.

金属によつて鋳造されたピストンを精密加工す
る場合には、直径の大きな連続繊維を複合する
と、機械加工が困難になり、従つてこのような連
続繊維の使用はかなり困難になる。これに対して
非結晶の短繊維は、その直径が細く、また繊維そ
のものも被削性に顕著な悪影響を及ぼさないため
に、十分に利用可能である。しかしこれらの繊維
集合体中に介在する粒状物、すなわちシヨツト
は、最大500μの直径を有してかなり大きなもの
があり、またこのシヨツトの含有量も繊維の20%
にも及び、直径が50〜150μのシヨツトがその大
半を占めるようになつている。従つてこのような
シヨツトは被削性に悪影響を及ぼし、機械加工を
困難にする。
In the precision machining of pistons cast from metal, the use of continuous fibers of large diameter makes machining difficult, and the use of such continuous fibers is therefore quite difficult. On the other hand, amorphous short fibers have a small diameter, and the fibers themselves do not have a significant adverse effect on machinability, so they can be fully utilized. However, the particulate matter, or shots, present in these fiber aggregates are quite large, with diameters of up to 500μ, and the content of these shots accounts for 20% of the fibers.
The majority of shots are now 50 to 150μ in diameter. Such shots therefore adversely affect machinability and make machining difficult.

そこで特開昭57−210140号は、繊維集合体中に
混在するシヨツトの大きさおよび量を規制し、
100メツシユ(最大直径149μ)以下のものを10重
量%以下にすることを提案している。しかしこの
提案によれば、直径が149μを越えるシヨツトを
10重量%以上含むことを許容し、また直径が
149μ未満のシヨツトについては、これを総て許
容することになる。
Therefore, Japanese Patent Application Laid-Open No. 57-210140 regulates the size and amount of shot mixed in the fiber aggregate,
It is proposed that the content of 100 meshes (maximum diameter 149μ) or less should be 10% by weight or less. However, according to this proposal, shots with a diameter exceeding 149μ
It is allowed to contain more than 10% by weight, and the diameter
All shots less than 149μ are permitted.

繊維によるピストンの複合強化は、複合される
位置に要求される目的をそれぞれ満足するもので
なければならず、例えばリング溝に複合される場
合にはこの溝に耐摩耗性を付与しなければなら
ず、また燃焼室の開口縁部に複合される場合に
は、この開口縁部に耐熱亀裂性を与えるものでな
ければならない。
Composite reinforcement of a piston with fibers must satisfy each purpose required for the position where it is composited, for example, when composited with a ring groove, this groove must be given wear resistance. First, when it is combined with the opening edge of the combustion chamber, it must provide heat cracking resistance to this opening edge.

セラミツク繊維中に含まれる粒状物、すなわち
シヨツトはセラミツク粒子から構成されることに
なるが、このシヨツトはピストンを構成するアル
ミニウム合金等の金属母材よりも高い硬さを有し
ており、あるいはまた摺動面を構成するシリンダ
ライナの表面のクロムメツキよりも高い硬さを有
している。従つて比較的大きなシヨツトを多く含
有する繊維をリング溝に複合した場合には、この
シヨツトが脱落して摺動面で自由に動くことにな
り、ピストンリングあるいはピストンがシリンダ
ライナに対して摺動する際の研摩材を構成するこ
とになり、かえつて摩耗を増加させることにもな
る。さらに無機繊維集合体が燃焼室の開口縁部に
複合される場合においても、比較的大きなシヨツ
トが含まれている短繊維を用いた場合には、十分
な耐熱亀裂性が得られないことが実験によつて確
認されている。すなわちシヨツトを含むものと除
去したものについて同一の条件で実験を試みたと
ころ、両者の間には大きな有意差が認められてい
る。
The particles contained in the ceramic fibers, that is, shots, are composed of ceramic particles, but these shots have a higher hardness than the metal base material such as aluminum alloy that makes up the piston, or It has higher hardness than the chrome plating on the surface of the cylinder liner that makes up the sliding surface. Therefore, if fibers containing many relatively large shots are composited into the ring groove, these shots will fall off and move freely on the sliding surface, preventing the piston ring or piston from sliding against the cylinder liner. This results in forming an abrasive material during polishing, which may even increase wear. Furthermore, even when inorganic fiber aggregates are composited at the opening edge of the combustion chamber, experiments have shown that sufficient heat cracking resistance cannot be obtained when short fibers containing relatively large shots are used. Confirmed by. In other words, when experiments were conducted under the same conditions for a sample containing shots and a sample from which shots were removed, a large significant difference was observed between the two.

本発明はこのような問題点に鑑みてなされたも
のであつて、ピストンのトツプリング溝あるいは
燃焼室の開口縁部に複合される無機繊維集合体中
に混在する粒状物、すなわちシヨツトの大きさを
所定の値以下に規制するとともに、その含有量に
ついても所定の値以下に規制するようにしたもの
であつて、これによつてシヨツトに起因する悪影
響を除去するようにした内燃機関用ピストンを提
供することを目的とするものである。
The present invention has been made in view of the above problems, and is aimed at reducing the size of particulate matter, that is, the size of shot, mixed in the inorganic fiber aggregate that is composited in the top ring groove of the piston or the opening edge of the combustion chamber. The piston for internal combustion engines is regulated to be below a predetermined value, and its content is also regulated to be below a predetermined value, thereby eliminating the adverse effects caused by the shot. The purpose is to provide

本発明の第1の特徴は、複合される無機繊維集
合体中に混在するシヨツトの大きさが8000メツシ
ユ以下に制限されていることである。この大きさ
はシヨツトの粒子の直径が最大11μ以下であるこ
とを示しており、これよりも大きなシヨツトは無
機繊維中には混在されないようにしたものであ
る。これは上述の如く、シヨツトが例えばセラミ
ツク粒子から成る場合には、アルミニウム合金あ
るいはシリンダライナの表面を構成するクロムメ
ツキよりも硬く、このためにこのシヨツトが脱落
した場合にはピストンリングとリング溝との間、
およびピストンリングとシンダライナとの間で研
摩材の作用をし、これによつて摩擦を増加させる
からである。なお11μ以下のシヨツトの場合に
は、その大きさは連続繊維の直径とほぼ等しいか
それよりも小さくなり、従つてこの程度のシヨツ
トはたとえ脱落しても、耐摩耗性をそれ程損うこ
とがないからである。
The first feature of the present invention is that the size of the shots mixed in the composite inorganic fiber aggregate is limited to 8000 mesh or less. This size indicates that the diameter of the shot particles is at most 11 μm or less, and shot particles larger than this are not mixed in the inorganic fibers. As mentioned above, if the shots are made of ceramic particles, for example, they are harder than aluminum alloy or the chrome plating that makes up the surface of the cylinder liner, and for this reason, if the shot falls off, the piston ring and ring groove will be damaged. while,
This is because it acts as an abrasive between the piston ring and the cinder liner, thereby increasing friction. In the case of shots of 11μ or less, the size is approximately equal to or smaller than the diameter of the continuous fiber, so even if shots of this size fall off, they will not significantly impair wear resistance. That's because there isn't.

また無機繊維中に含有を許容される8000メツシ
ユ以下のシヨツトについても、その量は極めて少
なく、面積比で0.001%以内に抑えられている。
面積比で0.001%というのは、ほぼ旨無に近いこ
とを示すものであつて、任意の断面について倍率
100倍の名刺判の写真を10枚貼り、その中に直径
が1mmの粒状物を1個許容する程度のものであ
る。複合される短繊維が結晶から成る無機繊維あ
るいはウイスカから構成される場合には、シヨツ
トをほぼ旨無にすることができるが、非結晶の短
繊維を使用する場合には出来るだけシヨツトが除
去されることが好ましく、完全に除去されないと
しても、面積比で0.001%以下にしなければなら
ない。
Furthermore, the amount of shots of 8000 mesh or less that is allowed to be contained in inorganic fibers is extremely small, and is suppressed to within 0.001% in terms of area ratio.
The area ratio of 0.001% means that it is almost insignificant, and the magnification of any cross section is
Ten 100x business card-sized photos are pasted, and one particle with a diameter of 1 mm is allowed in each photo. When the short fibers to be composited are composed of inorganic fibers made of crystals or whiskers, shots can be almost eliminated, but when amorphous short fibers are used, shots are removed as much as possible. Even if it is not completely removed, it should be reduced to 0.001% or less in terms of area ratio.

このような無機繊維維中に含まれる粒状物、す
なわちシヨツトの大きさおよび割合の制限は、こ
の無機繊維が燃焼室の開口縁部に複合される場合
においても適用される。このことは後述する試験
結果によつても証明されている。一般に燃焼室に
無機繊維が複合される場合は、この繊維が熱亀裂
に対する抗力を発揮することになるが、無機繊維
中にシヨツトが多く含有する場合には、このシヨ
ツトによつて上記の抗力が低減され、これによつ
て耐応力破壊の目的が達成されなくなるからであ
る。従つて内燃機関用のピストンのリング溝ある
いは燃焼室の開口縁部に無機繊維集合体を複合さ
せる場合には、第2図に示すような粒状物11を
混在している無機繊維10を用いることなく、第
3図に示すように粒状物11がほぼ完全に除去さ
れた無機繊維10を用いるようにしなければなら
ない。
Such restrictions on the size and proportion of particulate matter, ie, shots, contained in the inorganic fibers also apply when the inorganic fibers are composited at the opening edge of the combustion chamber. This is also proven by the test results described below. Generally, when inorganic fibers are combined in the combustion chamber, these fibers exert resistance against thermal cracking, but when the inorganic fibers contain a large amount of shot, the above resistance is exerted by these shots. This is because the stress fracture resistance is reduced, thereby defeating the purpose of stress fracture resistance. Therefore, when inorganic fiber aggregates are composited into the ring groove of a piston for an internal combustion engine or the opening edge of a combustion chamber, inorganic fibers 10 mixed with particulate matter 11 as shown in FIG. 2 should be used. Rather, as shown in FIG. 3, inorganic fibers 10 from which particulate matter 11 has been almost completely removed must be used.

つぎに本発明において複合される無機繊維集合
体の配列方向およびアスペクト比について述べ
る。これらの条件は、耐摩耗性を要求されるトツ
プリング溝と、耐熱亀裂性を要求される燃焼室の
開口縁部とでは異なつている。第4図はピストン
12のトツプリング溝13に無機繊維集合体14
を複合させた状態を示すものであつて、この複合
された無機繊維集合体14は、拡大すれば第5図
のようになる。このリング溝13にはピストンリ
ングが装着され、作動中にこのピストンリングの
外周面はシリンダライナと摺動することになる
が、このピストンリングの上面および下面はそれ
ぞれ無機繊維集合体14のZ−Z面と平行な面と
接触することになる。従つてとくにZ−Z面と平
行な面の耐摩耗性の向上が重要になつてくる。
Next, the arrangement direction and aspect ratio of the inorganic fiber aggregates composited in the present invention will be described. These conditions are different for the top ring groove, which requires wear resistance, and the opening edge of the combustion chamber, which requires heat crack resistance. FIG. 4 shows an inorganic fiber aggregate 14 in the top ring groove 13 of the piston 12.
The composite inorganic fiber aggregate 14 becomes as shown in FIG. 5 when enlarged. A piston ring is installed in this ring groove 13, and the outer circumferential surface of this piston ring slides on the cylinder liner during operation, but the upper and lower surfaces of this piston ring are connected to the Z-axis of the inorganic fiber aggregate 14, respectively. It will come into contact with a surface parallel to the Z plane. Therefore, it is especially important to improve the wear resistance of the surface parallel to the Z-Z plane.

一般に耐摩耗性を向上させるために異種材料を
複合強化する場合には、必ずしも繊維強化が最善
ではなく、粒子の分散効果の方がより好ましい。
すなわち例えば工具に使用される超硬材や耐熱材
料として使用されるサーメツト等がこれに該当す
る。従つてこのような観点から考察すれば、無機
繊維集合体を構成するそれぞれの繊維の直径に対
する長さの比、すなわちアスペクト比が小さい程
耐摩耗性の付与に貢献することになる。また第5
図におけるZ−Z面には、短繊維の外周面よりも
端面ができるだけ露出するような配列とすること
が好ましいことになる。
In general, when reinforcing dissimilar materials in a composite manner to improve wear resistance, fiber reinforcement is not necessarily the best, and the dispersion effect of particles is more preferable.
That is, examples of this include carbide materials used in tools and cermets used as heat-resistant materials. Therefore, when considered from this perspective, the smaller the ratio of the length to the diameter of each fiber constituting the inorganic fiber aggregate, that is, the smaller the aspect ratio, the more it contributes to imparting wear resistance. Also the fifth
In the Z-Z plane in the figure, it is preferable to arrange the short fibers so that the end faces are exposed as much as possible rather than the outer peripheral surfaces of the short fibers.

しかし本発明は短繊維が完全な方向性を持たず
に無機繊維集合体を構成するものを主として対象
としているので、このような場合におけるZ−Z
断面では第7図に示す繊維分布よりも、むしろ第
6図に示す繊維分布であることが好ましい。これ
に対してZ−Z面と直交するX−X面およびY−
Y面においては、第7図に示すような分布である
ことが好ましい。さらに本発明の好ましい実施態
様においては、トツプリング溝13に複合される
無機繊維集合体においては、トツプリング溝13
の表面に現われる無機繊維の内のアスペクト比が
100以下のものがその面に現われる繊維の面積の
70%以上になるように配列されていることであ
る。すなわちトツプリング溝に複合される場合に
は、無機繊維はなるべく短いものが用いられるよ
うにすればよい。
However, since the present invention is mainly intended for short fibers that do not have perfect directionality and constitute inorganic fiber aggregates, Z-Z in such cases
In the cross section, it is preferable to have the fiber distribution shown in FIG. 6 rather than the fiber distribution shown in FIG. 7. On the other hand, the X-X plane and the Y-
In the Y plane, it is preferable to have a distribution as shown in FIG. Furthermore, in a preferred embodiment of the present invention, in the inorganic fiber aggregate composited in the top ring groove 13, the top ring groove 13
The aspect ratio of the inorganic fibers appearing on the surface of
100 or less of the area of the fibers that appear on the surface
70% or more. That is, when the inorganic fibers are composited into the top ring groove, the inorganic fibers should be as short as possible.

つぎに無機繊維集合体15がピストン12の燃
焼室16の開口縁部に複合される場合には、第8
図に示すように無機繊維集合体15がリング状に
成形され、開口縁部に沿うように複合されること
になる。第9図はこの集合体15の一部を取出し
て拡大して示したものである。
Next, when the inorganic fiber aggregate 15 is composited on the opening edge of the combustion chamber 16 of the piston 12, the eighth
As shown in the figure, the inorganic fiber aggregate 15 is formed into a ring shape and is composited along the opening edge. FIG. 9 is an enlarged view of a part of this aggregate 15.

このような集合体15を構成する無機繊維10
の方向性について考察するに、この集合体15は
耐応力破壊を目的としている。従つて繊維の複合
則から明らかなように、同じ材質であつて同じ直
径の繊維を用いる場合には、短繊維より長繊維の
方が、また破壊を起こす応力の方向とのなす角度
が小さい程、さらに繊維の容積比が高い程大きな
効果をあげることができる。しかし連続繊維をそ
のまま、あるいはこれを切断した短繊維を使用す
る場合を除いては、繊維の方向を破壊に関与する
応力の方向と完全に一致するように配列すること
は困難である。しかしバラバラな短繊維から成る
集合体15によつて補強する場合には、この短繊
維がある範囲内において所定の配列がなされてい
ることを要する。
Inorganic fibers 10 constituting such an aggregate 15
Considering the directionality, this aggregate 15 is intended for stress fracture resistance. Therefore, as is clear from the composite law of fibers, when using fibers of the same material and the same diameter, long fibers are better than short fibers, and the smaller the angle with the direction of stress that causes fracture, the smaller the angle between the long fibers and the direction of stress that causes fracture. Furthermore, the higher the fiber volume ratio, the greater the effect. However, unless continuous fibers are used as they are or short fibers are used, it is difficult to arrange the fibers so that the direction of the fibers completely matches the direction of the stress involved in fracture. However, when reinforcing with the aggregate 15 made of discrete short fibers, the short fibers must be arranged in a predetermined range within a certain range.

第9図に示す無機繊維集合体15において、理
想的な繊維の配列は、第9図におけるX−X断面
およびZ−Z断面が第10図に示す如くになり、
またY−Y断面が第11図の如くになることであ
る。しかし短繊維から無機繊維集合体15を構成
することを前提とすれば、個々の繊維は有限の長
さを持ち、かつ大局的に見れば僅かな方向性を持
つに過ぎないので、このような場合には、X−X
断面およびZ−Z断面が第12図に示す如くにな
り、またY−Y断面が第13図に示す如くになれ
ばよい。強化の複合則から見ても、このようにす
ればX−X方向およびZ−Z方向がY−Y方向よ
りも強いことが十分に予想される。
In the inorganic fiber aggregate 15 shown in FIG. 9, the ideal fiber arrangement is such that the X-X cross section and Z-Z cross section in FIG. 9 are as shown in FIG.
Further, the Y-Y cross section is as shown in FIG. 11. However, assuming that the inorganic fiber aggregate 15 is constructed from short fibers, each fiber has a finite length and has only a slight directionality when viewed from a broader perspective. In case, X-X
The cross section and the Z-Z cross section may be as shown in FIG. 12, and the Y-Y cross section may be as shown in FIG. 13. Considering the composite law of reinforcement, it is fully expected that if this is done, the strength will be stronger in the X-X direction and the Z-Z direction than in the Y-Y direction.

さらに短繊維の成形体によつて燃焼室16の開
口縁部を複合して強化する場合には、用いられる
繊維のアスペクト比が2000以上のものでは製造時
の配列がそのまま残る。従つてこのような条件の
元においては、ある程度繊維に方向性が生ずる。
しかしこの方向性は製造条件に支配され、さらに
繊維間にもつれがあるので、使用条件による方向
性の選択は全くできないという不利な要素を含
む。そこで製造時の繊維のもつれを解くために、
繊維をアスペクト比が200程度となるように短く
切断する。そしてこの後に水中解縺、遠心分離、
ふるい分け等をすることによつて、並存するシヨ
ツトが分離できるとともに、遠心分離の際の遠心
力の作用のさせ方によつて、たとえ全部ではない
としても繊維に方向性を持たせることができる。
ピストンにおける部分複合に要求される特性によ
つて、この大局的に生ずる繊維の方向性を利用す
ることが可能になる。
Further, when the opening edge of the combustion chamber 16 is compositely reinforced with a molded article of short fibers, if the aspect ratio of the fibers used is 2000 or more, the arrangement at the time of manufacture remains as is. Therefore, under such conditions, some degree of directionality occurs in the fibers.
However, this directionality is controlled by the manufacturing conditions, and since the fibers are entangled, there is a disadvantageous element in that the directionality cannot be selected at all depending on the usage conditions. Therefore, in order to untangle the fibers during manufacturing,
Cut the fibers into short pieces with an aspect ratio of about 200. After this, underwater disintegration, centrifugation,
By sieving, etc., the coexisting shots can be separated, and by applying centrifugal force during centrifugation, it is possible to impart directionality to the fibers, even if not all of them.
The required properties of the partial composite in the piston make it possible to take advantage of this globally occurring fiber orientation.

そして本発明の好ましい実施態様においては、
燃焼室の開口縁部に複合される無機繊維集合体の
繊維は、この開口縁部の周方向の任意の断面に現
われる無機繊維の内のアスペクト比が50以上のも
のがその面に現われる繊維の面積の70%以上に配
列されていることである。すなわち燃焼室の開口
縁部に対する繊維の複合の場合には、長い繊維の
比率を高めるとともに、繊維の量をも多くするこ
とによつて耐熱亀裂性をより高めることができる
ようになる。
And in a preferred embodiment of the present invention,
The fibers of the inorganic fiber aggregate to be composited at the opening edge of the combustion chamber are those having an aspect ratio of 50 or more among the inorganic fibers appearing on any circumferential cross section of the opening edge. They must be arranged over 70% of the area. That is, in the case of composite fibers for the opening edge of the combustion chamber, the heat cracking resistance can be further improved by increasing the ratio of long fibers and increasing the amount of fibers.

つぎに本発明を具体的な実施例によつて説明す
る。
Next, the present invention will be explained using specific examples.

まず第1の実施例につき説明すると、酸化アル
ミニウム(Al2O3)95%、二酸化珪素(SiO2)5
%の繊維から成る無機繊維集合体14あるいは1
5によつて複合されたアルミニウム合金製のピス
トンについて、このピストンのトツプリング溝の
耐摩耗性および燃焼室の開口縁部の耐熱亀裂性に
関する試験を行なつた。なお耐摩耗性の試験は、
ピストン12の集合体14が複合された部分から
摩耗試験片を採取し、ピストンリングと同一の組
成の鋳鉄との滑り摩擦を行ない、その摩耗量を測
定している。
First, to explain the first example, aluminum oxide (Al 2 O 3 ) 95%, silicon dioxide (SiO 2 ) 5%
Inorganic fiber aggregate consisting of 14 or 1% fibers
Tests were conducted on the abrasion resistance of the top ring groove of the piston and the heat cracking resistance of the opening edge of the combustion chamber on the aluminum alloy piston composited by No. 5. In addition, the wear resistance test is
A wear test piece is taken from a part where the assembly 14 of the piston 12 is combined, and the amount of wear is measured by subjecting it to sliding friction with cast iron having the same composition as the piston ring.

また耐熱亀裂性に関する測定は、第14図に示
す装置によつて行なわれている。この装置は燃焼
室16の開口縁部に近接して配された加熱コイル
17によつてとくに燃焼室16の開口縁部を加熱
し、ついで空気パイプ18によつて冷却を行なう
装置である。そして第14図に示すグラフから明
らかなように、加熱コイル17によつて加熱する
場合には、燃焼室16の開口縁部が約350℃に加
熱される。この加熱および冷却のサイクルは第1
5図に示すようになつており、冷却時には約170
℃前後に燃焼室16の開口縁部が冷却されるよう
になつている。
Furthermore, measurements regarding heat cracking resistance were carried out using the apparatus shown in FIG. This device heats especially the opening edge of the combustion chamber 16 by means of a heating coil 17 disposed close to the opening edge of the combustion chamber 16, and then cools it by means of an air pipe 18. As is clear from the graph shown in FIG. 14, when heating is performed by the heating coil 17, the opening edge of the combustion chamber 16 is heated to approximately 350°C. This heating and cooling cycle
As shown in Figure 5, the temperature is approximately 170 when cooled.
The opening edge of the combustion chamber 16 is cooled to around .degree.

そして上記の耐摩耗性に関する試験の結果は第
16図においてDで示されており、酸化アルミニ
ウムと二酸化珪素とから成り、しかもシヨツトが
完全に除去された無機繊維集合体14によつて強
化されたトツプリング溝13は極めて低い摩耗量
を示している。なお第16図においてAで示すも
のは、アルミニウム合金から成るピストンについ
ての結果であり、全く繊維の強化が行なわれてい
ないものである。また同図においてBで示す結果
は、酸化アルミニウムと二酸化珪素とから成る無
機繊維集合体を用い、しかもこの集合体中からシ
ヨツトを除去しないものについての結果である。
また同図においてCで示す結果は、上述の特開昭
57−210140号で規制された範囲内の10%のシヨツ
トを含む場合の摩耗量を示している。なおここで
用いられている無機繊維集合体を構成する繊維の
太さは、150メツシユ以下が2%、200メツシユ以
下が3.5%、250メツシユ以下が2%、400メツシ
ユ以下が1.5%となつている。
The results of the above-mentioned abrasion resistance test are shown by D in FIG. 16, and are reinforced with an inorganic fiber aggregate 14 made of aluminum oxide and silicon dioxide, and from which shots have been completely removed. The top ring groove 13 exhibits extremely low wear. In addition, what is shown by A in FIG. 16 is the result for a piston made of an aluminum alloy, which is not reinforced with fibers at all. In addition, the results indicated by B in the figure are the results obtained using an inorganic fiber aggregate made of aluminum oxide and silicon dioxide, and in which shots were not removed from the aggregate.
In addition, the results indicated by C in the same figure are from the above-mentioned
It shows the amount of wear when 10% of shots are included within the range regulated by No. 57-210140. The thickness of the fibers constituting the inorganic fiber aggregate used here is 2% for 150 meshes or less, 3.5% for 200 meshes or less, 2% for 250 meshes or less, and 1.5% for 400 meshes or less. There is.

これらの結果から明らかなように、トツプリン
グ溝13を無機繊維集合体14によつて複合して
強化を図ろうとしても、シヨツトを含む場合やあ
るいはシヨツトの含有量が10%程度の場合には、
全く効果が生ずることがなく、複合による補強を
図らないアルミニウム合金から成るピストンより
も摩耗量が多くなつている。このことはシヨツト
が耐摩耗性を向上させる上で極めて悪い影響を及
ぼすことを明確に示すものであつて、耐摩耗性を
向上させるためには、シヨツトの大きさおよびそ
の含有量が厳格に規制されなければならないこと
を物語つている。
As is clear from these results, even if an attempt is made to strengthen the top ring groove 13 by compounding it with the inorganic fiber aggregate 14, it will not work if it contains shots or if the shot content is about 10%. ,
It has no effect at all and wears out more than a piston made of aluminum alloy without composite reinforcement. This clearly shows that shots have an extremely negative effect on improving wear resistance, and in order to improve wear resistance, the size of shots and their content must be strictly regulated. It tells the story of what must be done.

さらに本実施例の無機繊維集合体15によつて
燃焼室の開口縁部が補強されたピストン12の耐
熱亀裂性についての試験を行なつた結果を第17
図に示す。同図においてDで示す結果が本実施例
の結果であり、この結果はAおよびCで示す従来
のピストンに比べて、耐熱亀裂性が著しく向上し
ていることが明らかである。なおAとCの結果を
比較すれば、たとえシヨツトを10%含有していて
も繊維によつて補強されたものは、全く補強が図
られていないアルミニウム合金から成るピストン
の結果Aに比べて耐熱亀裂性は向上するものの、
CとDの結果を比較すれば明らかなように、同じ
く無機繊維によつて部分強化を図つても、シヨツ
トがない方が遥かに高い耐熱亀裂性を示すことに
なる。従つて耐熱亀裂性をピストンに付与する場
合においても、複合される無機繊維中におけるシ
ヨツトの量をできるだけ少なくするようにしなけ
ればならない。
Furthermore, the results of a test on the heat cracking resistance of the piston 12 whose opening edge of the combustion chamber was reinforced by the inorganic fiber aggregate 15 of this example are presented in the 17th section.
As shown in the figure. In the figure, the results indicated by D are the results of this example, and it is clear that the heat cracking resistance is significantly improved compared to the conventional pistons indicated by A and C. Comparing the results of A and C, even if it contains 10% shot, the fiber-reinforced piston has better heat resistance than result A, which is a piston made of aluminum alloy that is not reinforced at all. Although crackability improves,
As is clear from comparing the results of C and D, even if partial reinforcement is achieved using inorganic fibers, the one without shots exhibits much higher heat cracking resistance. Therefore, even when imparting heat cracking resistance to the piston, it is necessary to minimize the amount of shots in the composite inorganic fibers.

つぎに本発明の第2の実施例について説明す
る。この実施例は複合される繊維のアスペクト比
の効果について試験を行なつたものであつて、酸
化アルミニウム95%、二酸化珪素5%から成り、
しかもシヨツトを含まない繊維についての試験を
行なつたものである。そしてここではアスペクト
比が70以下の短い繊維が全体の繊維に対して80%
以上を占める面と、アスペクト比70以上の繊維が
全体の80%以上を占める面についての摩耗試験お
よび耐熱亀裂の試験を行なつている。
Next, a second embodiment of the present invention will be described. In this example, the effect of the aspect ratio of the composite fiber was tested, and it was made of 95% aluminum oxide and 5% silicon dioxide.
Furthermore, tests were conducted on fibers that did not contain shot. And here, short fibers with an aspect ratio of 70 or less account for 80% of the total fibers.
Abrasion tests and heat cracking tests are conducted on the surface where fibers with an aspect ratio of 70 or more account for 80% or more of the total fiber.

この結果によれば、アスペクト比が70以下の場
合の摩耗量は第16図においてEで示されてお
り、アスペクト比が70以上のものの結果が第16
図においてDで示されている。この結果から明ら
かなように、アスペクト比が70以下の短い繊維を
80%以上占める面は、アスペクト比が70以上の繊
維が80%以上を占める面に対して約1/2の摩耗量
になることが示される。すなわち耐摩耗性を向上
させるためには、その面におけるアスペクト比の
低い短い繊維が多く存在することが良好な結果を
もたらすことになる。
According to this result, the amount of wear when the aspect ratio is 70 or less is shown as E in Fig. 16, and the result when the aspect ratio is 70 or more is shown as E in Fig. 16.
It is indicated by D in the figure. As is clear from this result, short fibers with an aspect ratio of 70 or less
It is shown that the amount of wear on a surface that accounts for 80% or more is approximately 1/2 that of a surface that is 80% or more occupied by fibers with an aspect ratio of 70 or more. That is, in order to improve wear resistance, the presence of many short fibers with a low aspect ratio on that surface will bring about good results.

つぎに同じ条件での耐熱亀裂性の試験を行なつ
た結果は第17図においてEおよびDで示されて
おり、この場合においては逆にアスペクト比が70
以上の繊維がその面の全体の繊維に対して80%以
上を占める場合の方がアスペクト比が70以下の短
い繊維が全体の繊維に対して80%以上占める面の
約2倍の耐熱亀裂性を持つことが判明している。
従つて耐熱亀裂性を向上させるためには、アスペ
クト比の大きな繊維をより多くその面に存在させ
るようにすればよい。
Next, the results of a heat cracking resistance test under the same conditions are shown as E and D in Figure 17, and in this case, on the contrary, the aspect ratio was 70.
When fibers with an aspect ratio of 70 or less account for 80% or more of the total fibers on that surface, the heat cracking resistance is approximately twice as high as on a surface where short fibers with an aspect ratio of 70 or less account for 80% or more of the total fibers. It has been found that it has
Therefore, in order to improve the heat cracking resistance, it is sufficient to have more fibers with a large aspect ratio present on the surface.

つぎに本発明の第3の実施例を述べると、ここ
では0.8μの直径の炭化珪素のウイスカが用いられ
ており、このウイスカを用いて無機繊維集合体1
4,15をそれぞれ形成し、ピストン12に複合
させるようにした。このピストン12のトツプリ
ング溝13の摩耗および燃焼室16の開口縁部の
耐熱亀裂性に関する試験結果は、それぞれ第16
図および第17図においてFで示されている。こ
の結果から明らかなように、炭化珪素のウイスカ
によつて複合強化が図られたピストンは、トツプ
リング溝13の摩耗量が最も少なく、さらに燃焼
室16の開口縁部の亀裂も最も少なくなつてお
り、総ての試験の中で最高の成績を収めている。
これは集合体14,15を形成する短繊維が全く
シヨツトを含まない単結晶から構成されており、
しかもその直径および長さがそれぞれ非常に小さ
いことによるものと考えられる。
Next, a third embodiment of the present invention will be described. Here, a silicon carbide whisker with a diameter of 0.8μ is used, and this whisker is used to form an inorganic fiber aggregate.
4 and 15, respectively, and combined with the piston 12. The test results regarding the wear of the top ring groove 13 of the piston 12 and the heat crack resistance of the opening edge of the combustion chamber 16 are
It is indicated by F in the figure and FIG. As is clear from these results, the piston with composite reinforcement achieved by silicon carbide whiskers has the least amount of wear in the top ring groove 13 and also has the least amount of cracking at the opening edge of the combustion chamber 16. He achieved the highest score of all exams.
The short fibers forming the aggregates 14 and 15 are composed of single crystals that do not contain any shot.
Moreover, this is thought to be due to the fact that its diameter and length are both extremely small.

【図面の簡単な説明】[Brief explanation of drawings]

第1図は従来のアルミニウム合金から成るピス
トンを示す斜視図、第2図は本発明において複合
される無機繊維集合体であつて、シヨツトが含ま
れている状態の拡大断面図、第3図は同シヨツト
が除かれた状態の拡大断面図、第4図はトツプリ
ング溝の複合の状態を示すピストンの一部を破断
した斜視図、第5図はこのトツプリング溝に複合
される無機繊維集合体の斜視図、第6図および第
7図はこの無機繊維集合体の拡大断面図、第8図
はピストンの燃焼室の開口縁部の複合の状態を示
す一部を破断した斜視図、第9図はこの燃焼室の
開口縁部に複合される無機繊維集合体の斜視図、
第10図〜第13図はこの無機繊維集合体の拡大
断面図、第14図は繊維によつて複合されたピス
トンの耐熱亀裂性を測定するための装置の断面
図、第15図はこの装置によつて加えられる熱サ
イクルを示すグラフ、第16図は本発明の実施例
の非摩耗量の試験結果を示すグラフ、第17図は
本発明の実施例の耐熱亀裂性の試験結果を示すグ
ラフである。 なお図面に用いた符号において、10……無機
繊維、11……粒状物(シヨツト)、12……ピ
ストン、13……トツプリング溝、14,15…
…無機繊維集合体、16……燃焼室である。
Fig. 1 is a perspective view showing a conventional piston made of an aluminum alloy, Fig. 2 is an enlarged sectional view of the inorganic fiber aggregate composited in the present invention, including shots, and Fig. 3 is an enlarged sectional view of the inorganic fiber aggregate composited in the present invention. Fig. 4 is a partially cutaway perspective view of the piston showing the state in which the top ring groove is combined, and Fig. 5 is an inorganic fiber assembly combined in the top ring groove. 6 and 7 are enlarged cross-sectional views of this inorganic fiber aggregate, and FIG. 8 is a partially cutaway perspective view showing the composite state of the opening edge of the combustion chamber of the piston. Figure 9 is a perspective view of an inorganic fiber aggregate composited at the opening edge of this combustion chamber;
Figures 10 to 13 are enlarged cross-sectional views of this inorganic fiber aggregate, Figure 14 is a cross-sectional view of a device for measuring the heat crack resistance of a piston composited with fibers, and Figure 15 is a cross-sectional view of this device. FIG. 16 is a graph showing the test results of the non-wear amount of the example of the present invention, and FIG. 17 is a graph showing the test result of the heat cracking resistance of the example of the present invention. It is. In addition, in the symbols used in the drawings, 10... inorganic fiber, 11... granular material (shot), 12... piston, 13... top spring groove, 14, 15...
...Inorganic fiber aggregate, 16... Combustion chamber.

Claims (1)

【特許請求の範囲】 1 金属によつて鋳造されるとともに、その外周
面および頂面にそれぞれリング溝および凹部から
成る燃焼室を備えるピストンにおいて、前記リン
グ溝の内のトツプリング溝と前記燃焼室の開口縁
部の内の少なくとも一方に無機繊維集合体を複合
させるとともに、前記集合体を構成する無機繊維
が8000メツシユ(粒子の直径11μ)以上の粒状物
(シヨツト)を含有せず、しかも前記無機繊維中
に含有される8000メツシユ以下の粒状物の占める
面積が複合部の任意断面積の0.001%以下である
ことを特徴とする内燃機関用ピストン。 2 前記無機繊維集合体がトツプリング溝に複合
されるとともに、このトツプリング溝の表面に現
われる無機繊維の内のアスペクト比が100以下の
ものがその面に現われる繊維の占める面積の70%
以上になるように配列されていることを特徴とす
る特許請求の範囲第1項に記載の内燃機関用ピス
トン。 3 前記無機繊維集合体が燃焼室の開口縁部に複
合されるとともに、この開口縁部の周方向の任意
の断面に現われる無機繊維の内のアスペクト比が
50以上のものがその面に現われる繊維の面積の70
%以上になるように配列されていることを特徴と
する特許請求の範囲第1項に記載の内燃機関用ピ
ストン。 4 前記無機繊維集合体が結晶質のセラミツク繊
維から構成されることを特徴とする特許請求の範
囲第1項〜第3項の何れかに記載の内燃機関用ピ
ストン。 5 前記セラミツク繊維がセラミツクウイスカか
ら構成されることを特徴とする特許請求の範囲第
4項に記載の内燃機関用ピストン。
[Scope of Claims] 1. A piston that is cast from metal and has a combustion chamber consisting of a ring groove and a recess on its outer peripheral surface and top surface, respectively, wherein the top ring groove in the ring groove and the combustion chamber an inorganic fiber aggregate is composited on at least one of the opening edges of the inorganic fiber aggregate, and the inorganic fiber constituting the aggregate does not contain particles (shot) of 8000 meshes or more (particle diameter 11 μm), and A piston for an internal combustion engine, characterized in that the area occupied by particulate matter of 8000 mesh or less contained in the inorganic fiber is 0.001% or less of the arbitrary cross-sectional area of the composite part. 2. When the inorganic fiber aggregate is combined into the top ring groove, the inorganic fibers appearing on the surface of the top ring groove with an aspect ratio of 100 or less account for 70% of the area occupied by the fibers appearing on that surface.
The piston for an internal combustion engine according to claim 1, characterized in that the piston is arranged as described above. 3. The inorganic fiber aggregate is composited at the opening edge of the combustion chamber, and the aspect ratio of the inorganic fibers appearing in any circumferential cross section of the opening edge is
50 or more of the area of fibers that appear on its surface 70
% or more, the piston for an internal combustion engine according to claim 1. 4. A piston for an internal combustion engine according to any one of claims 1 to 3, wherein the inorganic fiber aggregate is composed of crystalline ceramic fibers. 5. The piston for an internal combustion engine according to claim 4, wherein the ceramic fiber is composed of a ceramic whisker.
JP7518483A 1983-04-28 1983-04-28 Piston used for internal-combustion engine Granted JPS59201953A (en)