JPH0249920A - Insert of auxiliary combustion chamber for diesel engine - Google Patents

Insert of auxiliary combustion chamber for diesel engine

Info

Publication number
JPH0249920A
JPH0249920A JP9603089A JP9603089A JPH0249920A JP H0249920 A JPH0249920 A JP H0249920A JP 9603089 A JP9603089 A JP 9603089A JP 9603089 A JP9603089 A JP 9603089A JP H0249920 A JPH0249920 A JP H0249920A
Authority
JP
Japan
Prior art keywords
combustion chamber
heat
insert
chamber insert
sub
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
JP9603089A
Other languages
Japanese (ja)
Inventor
Sakatoyo Sato
佐藤 栄豊
Tsutomu Hirayaku
平訳 勉
Makoto Suzuki
信 鈴木
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Riken Corp
Original Assignee
Riken Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Riken Corp filed Critical Riken Corp
Priority to JP9603089A priority Critical patent/JPH0249920A/en
Publication of JPH0249920A publication Critical patent/JPH0249920A/en
Ceased legal-status Critical Current

Abstract

PURPOSE:To enhance the heat resistance and thermal fatigue resistance of an aux. combustion chamber insert by combining a metal or alloy having a higher thermal conductivity than the body of the insert with the periphery of a part of or the whole flange of the insert. CONSTITUTION:The body 1 of an aux. combustion chamber insert provided with a jet 2 at its bottom is made of an uncostly heat resistant steel having heat resistance in a certain degree, and in the manufacturing process thereof a part of or the whole periphery of a flange part is combined with a metal having a very large thermal conductivity such as Cu or Cu alloy. Such metal in the form of e.g. a pin 5 is driven in the periphery of the flange 3. A ring- shaped groove is provided in the periphery of the flange 3, and there a metal with very large thermal conductivity is fillet welded. This enables release of the heat from insert body effectively to the outside and enhances the heat resistance and thermal fatigue resistance.

Description

【発明の詳細な説明】 (産業上の利用分野) 本発明は、ディーゼルエンジン用副燃焼室インサートの
改良に係り、更に詳しくは、副燃焼室インサートの外周
部の全周若しくは一部に熱伝導率の良い金属若しくは合
金を組合せることにより、耐久性の向上を図ったディー
ゼルエンジン用副燃焼室インサートに関する。
Detailed Description of the Invention (Field of Industrial Application) The present invention relates to an improvement in a sub-combustion chamber insert for a diesel engine, and more specifically, the present invention relates to an improvement in a sub-combustion chamber insert for a diesel engine. This invention relates to a sub-combustion chamber insert for a diesel engine that has improved durability by combining metals or alloys with high efficiency.

(従来の技術) 従来の金属製副燃焼室インサートに使用される材料とし
ては耐酸化性、高温強度、耐ヒートチェツク性、耐熱疲
労性等が要求されており5UH3,5UH616等のマ
ルテンサイト系耐熱鋼、5UH310,5UH309等
のオーステナイト系耐熱鋼、NIMONIC80A、L
CN−155等の超耐熱合金がある。
(Prior art) Materials used for conventional metal sub-combustion chamber inserts are required to have oxidation resistance, high temperature strength, heat check resistance, thermal fatigue resistance, etc., and martensitic heat resistant materials such as 5UH3 and 5UH616 are required. Steel, austenitic heat-resistant steel such as 5UH310, 5UH309, NIMONIC80A, L
There are super heat-resistant alloys such as CN-155.

(発明が解決しようとする課題) 最近ディーゼルエンジンは小型化および熱効率の向上、
高速回転の要求が強く、そのために燃焼室周辺の熱負荷
が大きくならざるを得ない。その結果、5UH3,5U
H61,6等のマルテンサイト系耐熱鋼は熱膨張率が小
さく耐熱疲労性、耐ヒートチエツク性に優れているが、
耐酸化性、高温強度が劣り、最近の高負荷エンジンの使
用に耐えられなくなってきている。又、5UH310,
5UH309等のオーステナイト系耐熱鋼はマルテンサ
イト系、フェライト系耐熱鋼に較べ高温強度は大きいが
、高温時に発生する熱応力を抑えるに充分でなく耐ヒー
トチエツク性、耐変形性に劣る。
(Problem to be solved by the invention) Recently, diesel engines have become smaller and have improved thermal efficiency.
There is a strong demand for high-speed rotation, which inevitably increases the heat load around the combustion chamber. As a result, 5UH3,5U
Martensitic heat-resistant steels such as H61, 6 have a small coefficient of thermal expansion and are excellent in thermal fatigue resistance and heat check resistance.
It has poor oxidation resistance and high-temperature strength, and is no longer able to withstand the use of modern high-load engines. Also, 5UH310,
Although austenitic heat-resistant steels such as 5UH309 have higher high-temperature strength than martensitic and ferritic heat-resistant steels, they are not sufficient to suppress thermal stress generated at high temperatures and are inferior in heat check resistance and deformation resistance.

NIMONIC80A、LCN−155等の超耐熱合金
は耐酸化性、高温強度において優れ熱応力に対しては充
分に耐え耐変形性もあるが、一般に500〜700℃に
おける靭性が劣り、それ以上の高温からのエンジンの冷
却時の引張り応力に対する変形に追従できず、5UH3
10,5UH309等のオーステナイト系耐熱鋼に較べ
ても耐ヒートチエツク性、耐熱疲労性に劣る。更に高価
な合金元素を多量に含有する高合金になればなる程材料
価格面に不利であり非常に高コストとなる。
Super heat-resistant alloys such as NIMONIC 80A and LCN-155 have excellent oxidation resistance and high-temperature strength, and can withstand thermal stress sufficiently and are resistant to deformation. Unable to follow the deformation due to tensile stress during cooling of the engine, 5UH3
Even compared to austenitic heat-resistant steels such as 10,5UH309, it has poor heat check resistance and thermal fatigue resistance. Furthermore, the higher the alloy containing a large amount of expensive alloying elements, the more disadvantageous it becomes in terms of material cost, and the cost becomes extremely high.

(課題を解決するための手段) 本発明は上述した副燃焼室インサートの特異性に着目し
、熱伝導を高め副燃焼室の熱の放出を増進させて、耐久
性の向上を図った副燃焼室インサートを安価に提供する
ことを目的とする。
(Means for Solving the Problems) The present invention focuses on the specificity of the above-mentioned sub-combustion chamber insert, and improves the durability of the sub-combustion chamber by increasing heat conduction and promoting heat release from the sub-combustion chamber. The purpose is to provide chamber inserts at low cost.

上3dの目的を達成するために本発明は、副燃焼室イン
サート本体をある程度の耐熱性を有する安価な耐熱鋼で
製造し、その製造過程において鍔部の外周部の全周若し
くは一部に、銅或いは銅合金等の熱伝導率の非常に大き
い金属を組合せることによって、例えば、鍔外周部に熱
伝導率の非常に大きい金属をピンとして打ち込む、また
は、鍔部の外周部に環状溝を設けて全周に熱伝導率の非
常に大きい金属を肉盛り溶接を行なうことによって副燃
焼室インサート本体の熱を外部に、より効果的に放出す
る耐久性に優れた副燃焼室インサートを安価に提供する
。
In order to achieve the above object (3d), the present invention manufactures the sub-combustion chamber insert main body from inexpensive heat-resistant steel that has a certain degree of heat resistance, and in the manufacturing process, the entire circumference or a part of the outer periphery of the flange is coated with By combining metals with very high thermal conductivity such as copper or copper alloys, for example, by driving a metal with very high thermal conductivity as a pin into the outer periphery of the flange, or by creating an annular groove on the outer periphery of the flange. By overlaying and welding a metal with extremely high thermal conductivity around the entire circumference, we have created a highly durable sub-combustion chamber insert that releases heat from the sub-combustion chamber insert body to the outside more effectively at a low price. provide.

又、副燃焼室インサート本体をある程度の耐熱性を有し
熱変形の少ないマルテンサイト系の5UH−3,5UH
616等の耐熱鋼で形成し、異常に加熱される噴口の周
縁部を耐熱疲労性に優れたLCN−155等の超耐熱合
金で成形して組合せ、更に、噴口の周縁部から早く熱を
逃すために、鍔外周部から噴口周縁部近傍に至る環状溝
を設けて熱伝導率の高い銅或いは銅合金を肉盛り溶接を
行うことによって、副燃焼室インサート本体の熱を外部
により効果的に放出しインサート全体の変形を少なくシ
、耐熱使用温度を向上させてより耐久性に優れた副燃焼
室インサートを安価に提供する。
In addition, the main body of the sub-combustion chamber insert is made of martensitic material 5UH-3,5UH, which has a certain degree of heat resistance and less thermal deformation.
It is made of heat-resistant steel such as 616, and the periphery of the nozzle, which gets abnormally heated, is molded and combined with a super heat-resistant alloy such as LCN-155, which has excellent heat fatigue resistance, and furthermore, heat is quickly dissipated from the periphery of the nozzle. In order to do this, an annular groove is created from the outer periphery of the flange to the vicinity of the periphery of the nozzle, and by overlaying copper or copper alloy with high thermal conductivity, the heat from the main body of the sub-combustion chamber insert is released more effectively to the outside. To inexpensively provide a sub-combustion chamber insert which has excellent durability by reducing deformation of the entire insert and improving its heat-resistant operating temperature.

(実施例) 以下、本発明を実施例の図面に基づいて具体的に説明す
る。
(Example) Hereinafter, the present invention will be specifically described based on drawings of examples.

第1実施例 第1図から第4図に示すように副燃焼室インサート本体
1を、5US310Sと第2表に示す化学成分を有する
RIK−45Nで冷間鍛造によって製造し、その製造過
程において副燃焼室インサート本体1の鍔部3に、第1
表の組合せに示すように、銅からなるピン5を打ち込ん
だものと銅を肉盛り溶接したものを、第5図に示す製造
方法によって製造した。
FIRST EXAMPLE As shown in FIGS. 1 to 4, the auxiliary combustion chamber insert body 1 is manufactured by cold forging from 5US310S and RIK-45N having the chemical composition shown in Table 2. A first
As shown in the combinations in the table, one in which a copper pin 5 was driven and one in which copper was welded overlay were manufactured by the manufacturing method shown in FIG.

第1表 第2表       (重態%) ■インサート本体1を5US310Sまたは、RIK4
5Nより冷間鍛造によって成形した。
Table 1 Table 2 (Severe condition %) ■Insert body 1 is 5US310S or RIK4
It was formed by cold forging from 5N.

■機械加工により、鍔部3の外周部に銅ピン5を打ち込
むための直径2.5〜3 mm X長さ3mmのピン孔
4を穿孔、或いは、肉盛り溶接するため巾2.5〜3m
mX深さ2.5〜3mmの環状溝6を形成する。
■By machining, a pin hole 4 with a diameter of 2.5 to 3 mm and a length of 3 mm is drilled for driving a copper pin 5 into the outer periphery of the flange 3, or a width of 2.5 to 3 m is used for overlay welding.
An annular groove 6 with a depth of 2.5 to 3 mm is formed.

次いで、第1図と第2図に示すように、ピン孔4に銅ピ
ン5を打ち込み、又は、第3図と第4図に示すように環
状溝6に銅の肉盛り溶接を行なった後、 ■機械加工等の処理を行ない所定の寸法に仕上げる。
Next, as shown in FIGS. 1 and 2, a copper pin 5 is driven into the pin hole 4, or as shown in FIGS. 3 and 4, copper is overlaid welded into the annular groove 6. , ■Perform processing such as machining to finish to the specified dimensions.

上記方法により形成された副燃焼室インサートを耐熱疲
労試験片として耐熱疲労試験を行なった。
A heat fatigue test was conducted using the sub-combustion chamber insert formed by the above method as a heat fatigue test piece.

尚、比較品として5US310S材のみによる副燃焼室
インサートを用いて行なった。
As a comparative product, a sub-combustion chamber insert made only of 5US310S material was used.

耐熱疲労試験は第6図に示す試験装置10に取付【プら
れた第7図に示す保持具11に試験片の副燃焼室インサ
ート本体1を固定し、ガスバーナ12で下面から約90
0℃に加熱した後、試験装置10を回転させ副燃焼室イ
ンサート本体1をスプレー13の上方に移動させて水を
スプレーして約40℃まで水冷した後空冷する。第8図
に示す加熱、冷却のサイクルを300回繰り返したのち
。
The thermal fatigue test was carried out by fixing the auxiliary combustion chamber insert body 1 of the test piece to the holder 11 shown in FIG. 7, which was attached to the testing apparatus 10 shown in FIG.
After heating to 0° C., the test device 10 is rotated, the auxiliary combustion chamber insert main body 1 is moved above the spray 13, and water is sprayed to cool it to about 40° C., followed by air cooling. After repeating the heating and cooling cycle shown in FIG. 8 300 times.

第9図に示すように噴口部2の底面周縁に発生した亀裂
16の長さを測定し、その長さの合計によって耐熱疲労
性を判定した。
As shown in FIG. 9, the length of the crack 16 generated at the bottom periphery of the nozzle 2 was measured, and the thermal fatigue resistance was determined based on the total length.

亀裂の長さの測定結果を第1表に併記した。The measurement results of the crack lengths are also listed in Table 1.

第1表から明らかなように、比較品のSUS 310S
材のみからなるものは亀裂の長さは15mmであったの
に対して、副燃焼室インサートを5O5310Sで形成
し銅のピンを打ち込んだもの(試料番号IA)は8mm
、銅の肉盛り溶接を行なったもの(試料番号IB)は5
mmと耐熱疲労性の改善が認めらる。
As is clear from Table 1, the comparative product SUS 310S
The length of the crack was 15 mm for the one made of wood only, whereas the length of the crack was 8 mm for the one in which the auxiliary combustion chamber insert was made of 5O5310S and a copper pin was driven in (sample number IA).
, the one with copper overlay welding (sample number IB) is 5.
Improvements in thermal fatigue resistance and thermal fatigue resistance were observed.

更に、副燃焼室インサートをRIK45Nで形成し、銅
ピンを打ち込んだもの(試料番号11A)は8+111
6、銅肉盛り溶接を行なったもの(試料番号■B)では
亀裂は認められず、耐熱疲労性が著しく向上し改善され
たことが認められる。
Furthermore, the sub-combustion chamber insert is made of RIK45N and a copper pin is driven into it (sample number 11A), which is 8+111.
6. No cracks were observed in the sample in which copper overlay welding was performed (sample number ■B), indicating that the thermal fatigue resistance was significantly improved.

なお、熱伝導率の優れた金属または合金を組合せるのは
本実施例のピンの打ち込みと肉盛り溶接に限定されるも
のでなく、副燃焼室インサートの形状、使用条件等によ
り適宜慣用の組合せ方を用いることは自在である。
Note that the combination of metals or alloys with excellent thermal conductivity is not limited to the pin driving and build-up welding of this example, but may be combined with any conventional combination as appropriate depending on the shape of the sub-combustion chamber insert, usage conditions, etc. You are free to use either method.

3外周部より噴孔2周縁近傍に至る部分に機械加工で環
状溝26を形成して、■TIG溶接法にて銅25を肉盛
りし、■最後に噴孔2を機械加工で形成して仕上げ加工
を行い、第11図に示すような副燃焼室インサートを得
た。
3. An annular groove 26 is formed by machining from the outer periphery to the vicinity of the periphery of the nozzle hole 2, ■ copper 25 is built up using the TIG welding method, and ■ finally the nozzle hole 2 is formed by machining. Finishing was performed to obtain a sub-combustion chamber insert as shown in FIG.

得られた副燃焼室インサートについて下記の試験を行な
った。
The following tests were conducted on the obtained auxiliary combustion chamber insert.

(1)加熱試験 (2)熱疲労試験 (3)熱へたり試験 第2実施例 第12図の製造工程図に示す如く、■インサート本体1
を5US403より冷間鍛造法にて成形し、噴孔2の周
縁部に四部20.21を同時付加加工しくA)、■ショ
ク(〜ブラストで凹部20.21の表面を清浄にし■L
CN−155の超耐熱合金をプラズマアーク溶接法によ
り肉盛溶接し超耐熱合金層22.23を形成後(B)■
1150’CX2H→急冷で固溶化熱処理を実施する。
(1) Heating test (2) Thermal fatigue test (3) Thermal fatigue test Second example As shown in the manufacturing process diagram in Figure 12, ■ Insert main body 1
Formed from 5US403 by cold forging method, and simultaneously added four parts 20.21 to the periphery of the nozzle hole 2.
After welding CN-155 super heat resistant alloy by plasma arc welding to form super heat resistant alloy layers 22 and 23 (B) ■
1150'CX2H → Implement solution heat treatment by rapid cooling.

■鍔(1)加熱試験 第13図に示す如く、インサート本体1をシリンダーヘ
ッド材質と同じAQ合金製ホルダー30に固定し、一定
条件でガスバーナー31にて夫々15.20.25秒間
加熱し、インサート噴孔2鋭角部の近傍に挿入した熱電
対32で温度を測定した。比較品として銅肉盛りを行わ
ない試料について同様な試験を行なった。その結果を第
1表に示す。
■Brim (1) Heating test As shown in Figure 13, the insert body 1 was fixed to a holder 30 made of AQ alloy, which is the same material as the cylinder head material, and heated under certain conditions with a gas burner 31 for 15, 20, and 25 seconds, respectively. The temperature was measured with a thermocouple 32 inserted near the acute corner of the insert nozzle hole 2. As a comparative product, a similar test was conducted on a sample without copper overlay. The results are shown in Table 1.

第1表 (℃) 試験結果を第2表に示す。Table 1 (℃) The test results are shown in Table 2.

第2表 第1表から明らかなように、本発明の銅肉盛を行なった
ものは最高温度が比較量の銅肉盛りを行わないものに比
して約20〜40℃低く1本発明品の放熱効果が大であ
ることが認められた。
As is clear from Table 2 and Table 1, the maximum temperature of the products with the copper overlay of the present invention is approximately 20 to 40°C lower than that of the products without the comparative amount of copper overlay. It was recognized that the heat dissipation effect was large.

(2)熱疲労試験 第1実施例と同一の試験装置及び試験方法によって、噴
孔部の周縁部に発生したクラック16の長さを測定し、
その長さの合計で耐熱疲労性を判定した。
(2) Thermal fatigue test The length of the crack 16 that occurred at the periphery of the nozzle hole was measured using the same test equipment and test method as in the first example,
Thermal fatigue resistance was determined based on the total length.

尚、比較量として従来のインサート本体をLCN−15
5で製作したもの(試料番号l)とインサート本体を5
US403で形成し、噴孔周縁部をLCN−155で肉
盛り溶接したもの(試料番号■)を作成し試験した。
For comparison, the conventional insert body was replaced with LCN-15.
The one manufactured in step 5 (sample number l) and the insert body in step 5
A sample (sample number ■) made of US403 and having the peripheral edge of the nozzle hole welded with LCN-155 was prepared and tested.

第2表から明らかなように、比較量!のLCN−155
一体型の亀裂長さが12n+m、比較量11の5US4
03にLCN−155を肉盛りしたもの11mmに対し
、本発明品の銅を肉盛りしたものは6ffnと約半分の
長さで耐熱疲労性が著しく向上し、改善されたことが認
められた。
As is clear from Table 2, the comparative amount! LCN-155
5US4 with integrated crack length of 12n+m and comparative amount of 11
03 with LCN-155 built-up, the length of the product of the present invention with copper built-up was 6ffn, which was about half the length, and it was recognized that the heat fatigue resistance was significantly improved.

(3)熱へたり試験 熱疲労試験を行った試料について第14図に示す底部平
面部のへたり量t(第11図c−c線上)を測定して耐
熱へたり性を評価した。
(3) Heat Settling Test For the samples subjected to the heat fatigue test, the heat settability was evaluated by measuring the settling amount t (on line c-c in Figure 11) of the bottom flat part shown in FIG. 14.

測定結果は、比較量■のLCN−155一体型のもの0
.2+mに対し、比較量■の5US403にLCN−1
55を肉盛りしたものは0.03mmと大巾に改善され
ているが本発明品の銅を肉盛りしたものは0.01+n
mと更に小さく、著しく耐熱へたり性が改善されており
放熱効果が認められた。
The measurement results are for the LCN-155 integrated type with comparative amount ■ 0
.. 2+m, LCN-1 to 5US403 of comparative amount ■
The width of the product with built-up copper of the present invention is 0.03mm, which is significantly improved, but the width of the product with built-up copper of the present invention is 0.01+n.
The heat dissipation effect was found to be even smaller than m, and the heat-setting resistance was significantly improved.

(効果) ディーゼルエンジン用副燃焼室インサートの鍔部外周部
の全周又は一部を熱伝導率の高い金属または合金を組合
せることにより、熱伝導率を高め、熱を外部に効率的に
放出し耐熱性、耐熱疲労性に優れ耐久性の向上が図られ
た副燃焼室インサートを安価に得られたこと、更に、噴
日周織部を肉盛り溶接によって超耐熱合金で構成するこ
とによりより耐久性の向上が図られた実用上の効果は顕
著である。
(Effect) By combining a metal or alloy with high thermal conductivity for the entire circumference or part of the outer circumference of the flange of the sub-combustion chamber insert for diesel engines, thermal conductivity is increased and heat is efficiently released to the outside. We were able to obtain a sub-combustion chamber insert at a low cost that has excellent heat resistance and thermal fatigue resistance, and improved durability.Furthermore, we have made the insert of the auxiliary combustion chamber with a super heat-resistant alloy by build-up welding the welding part of the weave, making it even more durable. The practical effect of improving performance is remarkable.

【図面の簡単な説明】[Brief explanation of the drawing]

第1図 本発明の第1実施例のピンを打ち込んだ副燃焼
室インサートの半断面図 第2図 第1図のA−A矢視断面図 第3図 本発明の第1実施例の肉盛り溶接をした副燃焼
室インサートの半断面図 第4図 第2図のB−B矢視断面図 第5図 本発明品の第1実施例の製造方法を示す工程図 第6図 熱疲労試験装置の概要図 第7図 熱疲労試験装置の試験片保持具と試験方法を示
す概要図 第8図 熱疲労試験の加熱冷却サイクルを示すグラフ図 第9図 亀裂の発生状況を示す平面図 第10図 本発明の第2実施例の副燃焼室インサートの
断面図 第11図 本発明の第2実施例の他の例を示す副燃焼室
インサートの断面図 第12図 本発明の第2実施例の製造方法を示す工程図 第13図 加熱試験方法を示す概要図 第14図 熱へたり量の?llllll在方法断面図1
=副燃焼室インサ一ト本体 2:噴口3:鍔部   4
:ピン孔  5:銅ビン6:環状溝 :銅肉盛り溶接部 10:熱疲労試験装置 1:治具 12 : ガスバーナ 13 ニ スプレー 16:亀裂 20゜ 21:凹部 22゜ 23:超耐熱合金肉盛り溶接部 25:銅肉盛り溶接部 26:環状溝 32:熱電対
Fig. 1 A half-sectional view of the auxiliary combustion chamber insert with a pin driven in according to the first embodiment of the present invention Fig. 2 A cross-sectional view taken along the line A-A in Fig. 1 Fig. 3 Overlay of the first embodiment of the present invention FIG. 4 is a half-sectional view of the welded auxiliary combustion chamber insert; FIG. 5 is a sectional view taken along the line B-B in FIG. 2; FIG. 5 is a process diagram showing the manufacturing method of the first embodiment of the product of the present invention; Figure 7 is a schematic diagram showing the test specimen holder of the thermal fatigue test device and the test method Figure 8 is a graph diagram showing the heating and cooling cycle of the thermal fatigue test Figure 9 is a plan view showing the state of crack occurrence Figure 10 FIG. 11 is a cross-sectional view of a sub-combustion chamber insert according to a second embodiment of the present invention. FIG. 12 is a cross-sectional view of a sub-combustion chamber insert showing another example of the second embodiment of the present invention. Manufacture of a second embodiment of the present invention Figure 13: Process diagram showing the method Figure 14: Schematic diagram showing the heating test method How much heat set? llllll method cross-sectional diagram 1
= Sub-combustion chamber insert body 2: Nozzle 3: Flange 4
: Pin hole 5: Copper bottle 6: Annular groove: Copper overlay welding part 10: Thermal fatigue test device 1: Jig 12: Gas burner 13 Nispray 16: Crack 20° 21: Recess 22° 23: Super heat resistant alloy overlay welding Part 25: Copper overlay welding part 26: Annular groove 32: Thermocouple

Claims (1)

【特許請求の範囲】 1、副燃焼室インサートの鍔部(3)の外周部の全周ま
たは一部に、インサート本体(1)に比較して熱伝導率
の高い金属若しくは合金を組合せたことを特徴とする耐
熱性、耐熱疲労性に優れたディーゼルエンジン用副燃焼
室インサート。 2、鍔部(3)の外周部にピン穴(4)を穿孔し熱伝導
率の高い金属若しくは合金からなるピン(5)を打ち込
んで組合せたことを特徴とする請求項1記載の耐熱性、
耐熱疲労性に優れたディーゼルエンジン用副燃焼室イン
サート。 3、鍔部(3)の外周部に環状溝(6)を設け、熱伝導
率の高い金属若しくは合金を肉盛り溶接によって組合せ
たことを特徴とする請求項1記載の耐熱性、耐熱疲労性
に優れたディーゼルエンジン用副燃焼室インサート。 4、副燃焼室インサート本体(1)をある程度の耐熱性
を有する耐熱鋼と超耐熱合金とを組合せたことを特徴と
する請求項1記載の耐熱性、耐熱疲労性に優れたディー
ゼルエンジン用副燃焼室インサート。
[Claims] 1. A metal or alloy having higher thermal conductivity than the insert body (1) is combined with the entire or part of the outer circumference of the flange (3) of the sub-combustion chamber insert. A sub-combustion chamber insert for diesel engines with excellent heat resistance and heat fatigue resistance. 2. Heat resistance according to claim 1, characterized in that a pin hole (4) is bored in the outer peripheral part of the flange (3) and a pin (5) made of a metal or alloy with high thermal conductivity is driven into the joint. ,
Sub-combustion chamber insert for diesel engines with excellent heat fatigue resistance. 3. Heat resistance and thermal fatigue resistance according to claim 1, characterized in that an annular groove (6) is provided on the outer periphery of the flange (3), and a metal or alloy with high thermal conductivity is combined by overlay welding. A secondary combustion chamber insert for diesel engines with excellent performance. 4. The sub-combustion chamber insert body (1) for a diesel engine having excellent heat resistance and thermal fatigue resistance according to claim 1, characterized in that the sub-combustion chamber insert main body (1) is made of a combination of heat-resistant steel having a certain degree of heat resistance and a super heat-resistant alloy. Combustion chamber insert.
JP9603089A 1988-05-09 1989-04-15 Insert of auxiliary combustion chamber for diesel engine Ceased JPH0249920A (en)