JPH03116830A - Etching back method - Google Patents
Etching back methodInfo
- Publication number
- JPH03116830A JPH03116830A JP25219089A JP25219089A JPH03116830A JP H03116830 A JPH03116830 A JP H03116830A JP 25219089 A JP25219089 A JP 25219089A JP 25219089 A JP25219089 A JP 25219089A JP H03116830 A JPH03116830 A JP H03116830A
- Authority
- JP
- Japan
- Prior art keywords
- etching
- insulating film
- film
- resist
- oxygen
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Abstract
(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。(57) [Summary] This bulletin contains application data before electronic filing, so abstract data is not recorded.
Description
【発明の詳細な説明】
[発明の目的]
(産業上の利用分野)
本発明は、半導体基板上回路の製造工程において配線上
に堆積された絶縁膜の表面を平坦化するためのエッチバ
ック方法に関する。[Detailed Description of the Invention] [Object of the Invention] (Industrial Application Field) The present invention provides an etch-back method for planarizing the surface of an insulating film deposited on wiring in the manufacturing process of a circuit on a semiconductor substrate. Regarding.
(従来の技術)
半導体集積回路では、高密度化、高集積化の要請からA
1等からなる多層配線が多用されている。こうした多層
配線構造を有する半導体集積回路の標準的な製造工程を
第1図(A)〜(C)を参照して次に説明する。まず、
予め素子が形成された半導体基板l上に第1の層間絶縁
膜2を堆積した後、A1層の蒸着、バターニングにより
第1層1配線3を形成する。つづいて、全面に第2の層
間絶縁膜4を堆積する。この時、第1図(A)に示すよ
うに下層の第1層1配線3の存在により該配線3間に対
応する前記第2の層間絶縁膜4部分に凹凸が形成され、
この状態で第2層AΩ配線を堆積すると前記凹凸による
段差により段切れを生じる。このため、同図(B)に示
すように第2の層間絶縁膜4を堆積した後、レジスト膜
5を表面が平坦になるように被覆する。次いで、前記レ
ジスト膜5から前記第2の層間絶縁膜4の表層に亘って
ドライエツチングしてエッチバックすることにより、同
図(C)に示すように第2の層間絶縁膜4表面を平坦化
する。この後、第2の層間絶縁膜上に第2層Ap配線(
図示せず)をAp層の蒸着、パターニングにより形成す
る。(Prior art) In semiconductor integrated circuits, due to the demand for higher density and higher integration, A
Multilayer wiring consisting of 1st grade wiring is often used. A standard manufacturing process for a semiconductor integrated circuit having such a multilayer wiring structure will now be described with reference to FIGS. 1(A) to 1(C). first,
After depositing a first interlayer insulating film 2 on a semiconductor substrate l on which elements have been formed in advance, a first layer 1 wiring 3 is formed by vapor deposition and patterning of an A1 layer. Subsequently, a second interlayer insulating film 4 is deposited over the entire surface. At this time, as shown in FIG. 1(A), due to the presence of the underlying first layer 1 wiring 3, unevenness is formed in the portion of the second interlayer insulating film 4 corresponding between the wirings 3,
If the second layer AΩ wiring is deposited in this state, a step break will occur due to the step difference due to the unevenness. For this reason, after depositing the second interlayer insulating film 4, as shown in FIG. 2B, a resist film 5 is coated so that the surface becomes flat. Next, by performing dry etching and etching back from the resist film 5 to the surface layer of the second interlayer insulating film 4, the surface of the second interlayer insulating film 4 is planarized as shown in FIG. do. After this, the second layer Ap wiring (
(not shown) is formed by vapor deposition and patterning of an Ap layer.
ところで、上述したレジスト膜と第2の層間絶縁膜をエ
ッチバックするに際してはエツチングの途中工程でレジ
ストと絶縁膜とが同一平面に露出し、最終表面を平坦化
するにはそれらを同時にエツチングすることが必要なた
め、それらレジストと絶縁膜(通常;5in2)のエツ
チング速度が等しい条件でドライエツチングすることが
要求される。このため、従来ではフロンガスと酸素との
混合ガスを用いて行っている。即ち、CF4のようなフ
ロン単独でドライエツチングすると、レジストに比べて
5IO2のエツチング速度が高くなって良好なエッチバ
ックを行えなくなる。これに対し、CF4に酸素を添加
することによりレジストのエツチング速度が大きくなる
ため、レジスト膜と5in2からなる絶縁膜の両者のエ
ツチング速度が等しくなる。By the way, when etching back the resist film and the second interlayer insulating film mentioned above, the resist and the insulating film are exposed on the same plane during the etching process, and in order to flatten the final surface, it is necessary to etch them at the same time. Therefore, dry etching is required under conditions where the etching rates of the resist and the insulating film (usually 5 in 2 ) are the same. For this reason, conventionally, a mixed gas of fluorocarbon gas and oxygen is used. That is, when dry etching is performed using a fluorocarbon such as CF4 alone, the etching speed of 5IO2 becomes higher than that of resist, making it impossible to perform a good etchback. On the other hand, since the etching rate of the resist increases by adding oxygen to CF4, the etching rates of both the resist film and the 5in2 insulating film become equal.
上述したCF4と酸素の混合ガスを用いたエツチングに
おいて、レジストHと5in2からなる絶縁膜のエツチ
ング速度の酸素添加量依存性は第4図に示す特性図とな
る。この第4図から明らかなようにCF4単独では、5
IO2からなる絶縁膜のエツチング速度が高く、酸素添
加量の増加に伴ってレジストのエツチング速度が増加す
る。そして、混合ガス中の酸素添加比率が3(196(
C点)になると両者のエツチング速度が等しくなる。し
かしながら、既述した第1図(A)〜(C)に示すエッ
チバック工程ではエツチングの進行に伴ってレジスト膜
の面積が減少し、SiO2からなる層間絶縁膜の露出面
積が増大する。5in2のエツチング生成物は、よく知
られているようにSiF4と02である。従って、酸素
量の添加制御によりレジストと絶縁膜のエツチング速度
を等しく設定してもエツチングが進行するに伴ってエツ
チング雰囲気中の酸素量が増大するのと等しいエツチン
グ挙動〆示す。このようなエツチング挙動は、第4図に
示すレジストと絶縁膜のエツチング速度が等しくなるC
点を外れて、両者のエツチング速度差が極端に大きくな
る領域でエツチングが進行することになる。その結果、
従来のCF4と酸素の混合ガスによるエッチバック法で
はエツチング中にレジスト膜と層間絶縁膜とのエツチン
グバランスが極端に崩れてしまうため、層間絶縁膜の表
面を平坦化できず、第2層Ag配線を形成する際に段切
れを生じるという問題があった。In the etching using the above-mentioned mixed gas of CF4 and oxygen, the dependence of the etching rate of the insulating film consisting of resist H and 5in2 on the amount of oxygen added is shown in the characteristic diagram shown in FIG. As is clear from this Figure 4, CF4 alone has a
The etching rate of the insulating film made of IO2 is high, and the etching rate of the resist increases as the amount of oxygen added increases. Then, the oxygen addition ratio in the mixed gas is 3 (196 (
At point C), the etching speeds of both become equal. However, in the etch-back process shown in FIGS. 1A to 1C, the area of the resist film decreases as the etching progresses, and the exposed area of the interlayer insulating film made of SiO2 increases. The 5in2 etching products are SiF4 and 02, as is well known. Therefore, even if the etching rates of the resist and the insulating film are set to be equal by controlling the amount of oxygen added, the etching behavior is the same as that of increasing the amount of oxygen in the etching atmosphere as etching progresses. Such etching behavior occurs at C, where the etching rates of the resist and insulating film are equal, as shown in FIG.
Etching progresses beyond this point in a region where the difference in etching speed between the two becomes extremely large. the result,
In the conventional etchback method using a mixed gas of CF4 and oxygen, the etching balance between the resist film and the interlayer insulating film is extremely disrupted during etching, so the surface of the interlayer insulating film cannot be flattened, and the second layer Ag wiring cannot be flattened. There was a problem in that step breakage occurred when forming.
なお、上記エッチバック対象である層間絶縁膜が燐添加
ガラス(PSG)、ボロン添加ガラス(B S G)等
のガラスからなる場合でも上述したのと同様な問題を生
じる。Note that even when the interlayer insulating film to be etched back is made of glass such as phosphorus-doped glass (PSG) or boron-doped glass (BSG), the same problem as described above occurs.
(発明が解決しようとする課題)
本発明は、上記従来の課題を解決するためになされたも
ので、エツチング中に同一平面内に露出した有機高分子
材料膜と酸化シリコン又はガラスからなる絶縁膜の面積
が変化してもそれらをほぼ等しい速度でエツチングし得
るエッチバック方法を提供しようとするものである。(Problems to be Solved by the Invention) The present invention has been made to solve the above-mentioned conventional problems. The object of the present invention is to provide an etch-back method that can etch them at approximately the same speed even if their areas change.
[発明の構成]
(課題を解決するための手段)
本発明は、半導体基板上に表面に凹凸を有する酸化シリ
コン又はガラスからなる絶縁膜を形成し、この絶縁膜上
に有機高分子材料膜をその表面か平坦になるように波頂
した後、前記有機高分子材料膜から前記絶縁膜の表層に
亘ってドライエツチングしてエッチバックする方法にお
いて、前記ドラエツチングをSF、を主エツチングガス
とし、これに水素又は酸素を添加した混合ガスを用いて
行うことを特徴とするものである。[Structure of the Invention] (Means for Solving the Problems) The present invention forms an insulating film made of silicon oxide or glass having an uneven surface on a semiconductor substrate, and forms an organic polymer material film on this insulating film. In the method of performing dry etching and etching back from the organic polymer material film to the surface layer of the insulating film after cresting the surface to make it flat, the dry etching is performed using SF as the main etching gas, This method is characterized by using a mixed gas to which hydrogen or oxygen is added.
上記ガラスとしては、例えば燐添加ガラス(PSG)、
ボロン添加ガラス(BSG)、ソーダガラスなどの低融
点ガラス等を用いることができる。Examples of the above-mentioned glass include phosphorous-doped glass (PSG),
Low melting point glasses such as boron-added glass (BSG) and soda glass can be used.
上記有機高分子材料としては、例えば半導体せ製造プロ
セスに汎用されている各種のレジスト、ポリイミド、ポ
リスチレン等を用いることができる。As the organic polymer material, for example, various resists, polyimide, polystyrene, etc., which are commonly used in semiconductor manufacturing processes, can be used.
上記SF、、に対する水素の添加量は、有機高分子材材
膜と絶縁膜を十分な速度でエツチングするること、両者
のエツチング速度を等しくすることから、40〜70%
、より好ましくは55〜BO%の範囲にすることが望ま
しい。The amount of hydrogen added to the above SF is 40 to 70% in order to etch the organic polymer material film and the insulating film at a sufficient rate and to make the etching speed of both the same.
, more preferably in the range of 55 to BO%.
上記SF6に対する酸素の添加量は、有機高分子材料膜
と絶縁膜を十分な速度でエツチングするること、両者の
エツチング速度を等しくすることから、5〜25%、よ
り好ましくは10〜15%の範囲にすることが望ましい
。The amount of oxygen added to the SF6 is 5 to 25%, more preferably 10 to 15%, in order to etch the organic polymer material film and the insulating film at a sufficient rate and to equalize the etching speed of both. It is desirable to set the range.
(作 用)
本発明者らは、SF6を主エツチングガスとし、これに
水素又は酸素を添加した混合ガスを用いることによって
、広いガス混合範囲で有機高分子材料膜と酸化シリコン
又はガラスからなる絶縁膜とのエツチング速度を等しく
できることを究明し、前記混合ガスにより有機高分子材
料膜及びその下に配置された前記絶縁膜の表層をエツチ
ングすることにより前記絶縁膜表面を平坦化できるエッ
チバック方法を見出した。以下、本発明のエッチバック
方法に用いられる混合ガスのエツチング特性について、
第2図及び第3図を参照して詳述する。(Function) By using SF6 as the main etching gas and a mixed gas with hydrogen or oxygen added thereto, the present inventors have succeeded in etching insulation made of an organic polymer material film and silicon oxide or glass in a wide range of gas mixtures. The inventors have discovered that the etching rate can be made equal to that of the film, and have developed an etch-back method that can planarize the surface of the insulating film by etching the organic polymer material film and the surface layer of the insulating film disposed thereunder using the mixed gas. I found it. The etching characteristics of the mixed gas used in the etchback method of the present invention will be explained below.
This will be explained in detail with reference to FIGS. 2 and 3.
第2図は、通常の平行平板型反応性イオンエツチング装
置を用い、SF6を40sccn+、エツチング圧力を
0.05torrs印加周波数をlW/Cff12の条
件でレジスト膜と酸化シリコン膜(プラズマCVD−5
iO2膜)をエツチングした場合におけるエツチング速
度の酸素添加依存性を示す。この第2図から明らかなよ
うに、SF6単独では酸化シリコン膜の方がレジスト膜
に比べてエツチング速度が高いが、それらのエツチング
速度差は前述したCF4に比べて小さい。これは、CF
4の場合には分解により生じたCF2等の不飽和な化学
種がレジスト表面にイオン衝撃により形成されたラジカ
ルサイトにアタックして重合するため、実質的なレジス
トエツチング速度は低くなる。これに対し、SF6の場
合にはその分解において前記レジスト表面に形成された
ラジカルサイトにアタックして重合する化学種が生成さ
れないため、CF4に比べてレジストエツチング速度が
高くなる。Figure 2 shows a photoresist film and a silicon oxide film (plasma CVD-5
3 shows the dependence of etching rate on oxygen addition when etching an iO2 film. As is clear from FIG. 2, when using SF6 alone, the etching rate of the silicon oxide film is higher than that of the resist film, but the difference in etching rate between them is smaller than that of CF4 described above. This is CF
In the case of No. 4, unsaturated chemical species such as CF2 generated by decomposition attack radical sites formed on the resist surface by ion bombardment and polymerize, so that the actual resist etching rate becomes low. On the other hand, in the case of SF6, chemical species that attack and polymerize the radical sites formed on the resist surface are not generated during its decomposition, so that the resist etching rate is higher than that of CF4.
一方、酸素を添加するとレジスト膜は酸素ラジカルによ
り酸化されるため、同第2図に示すようにエツチング速
度が増大し、酸化シリコン膜のエツチング速度と等しく
なる。また、酸化シリコン膜のエツチング速度の酸素添
加と共に増大する。On the other hand, when oxygen is added, the resist film is oxidized by oxygen radicals, so the etching rate increases as shown in FIG. 2 and becomes equal to the etching rate of the silicon oxide film. Furthermore, the etching rate of the silicon oxide film increases with the addition of oxygen.
これは、SF6の分解から生じたSFs 、SF4等の
化学種と酸化ラジカルとが反応し、Fラジカルを発生す
ることによるものである。CF4に比較してSF、、の
長所は、酸素添加に対してレジスト膜及び酸化シリコン
膜ともエツチング速度が増大し、エツチング速度が等し
い酸素添加範囲が拡大する点にある。このため、エツチ
ング途中で同一平面内に露出するレジスト膜、酸化シリ
コン膜の面積が変化し、酸化シリコン膜から発生する酸
素量が変化しても、両者のエツチング速度が高くなった
り、遅くなったりするものの、酸素添加比率15%を中
心にして±lθ%の範囲内では両者のエツチング速度差
がほとんど変化しないため、プロセスに対するマージン
を大きくできる。その結果、かかるSFl、に酸素を添
加した混合ガスにより前記レジスト膜から酸化シリコン
膜の表層に亘ってエッチバックすることにより、エツチ
ング途中での酸素の発生に伴ってそれら膜間のエツチン
グバランスが悪化することなく酸化シリコン膜の表面を
平坦化できる。This is because chemical species such as SFs and SF4 generated from the decomposition of SF6 react with oxidized radicals to generate F radicals. The advantage of SF, compared to CF4, is that the etching rate of both the resist film and the silicon oxide film increases with oxygen addition, and the range of oxygen addition where the etching rate is the same is expanded. Therefore, even if the areas of the resist film and silicon oxide film exposed in the same plane change during etching, and the amount of oxygen generated from the silicon oxide film changes, the etching speed of both may become higher or slower. However, within a range of ±lθ% around the oxygen addition ratio of 15%, the difference in etching rate between the two hardly changes, so the margin for the process can be increased. As a result, by etching back from the resist film to the surface layer of the silicon oxide film using a mixed gas containing oxygen added to the SFL, the etching balance between these films deteriorates as oxygen is generated during etching. The surface of the silicon oxide film can be flattened without any damage.
第3図は、通常の平行平板型反応性イオンエツチング装
置を用い、SF6を40scem、エツチング圧力を0
.05torr、印加周波数をIW/cm2の条件でレ
ジスト膜と酸化シリコン膜(プラズマCVD−3i02
膜)をエツチングした場合におけるエツチング速度の水
素添加依存性を示す。この第3図から明らかなように、
水素を添加するとレジスト膜、酸化シリコン膜ともにエ
ツチング速度が増大する。これは、SFb単独の場合に
はその放電から生じるSが表面に堆積してエツチングを
抑制するが、水素を添加することにより水素ラジカルが
Sと反応して硫化水素(H2S)を生成してSを除去す
るためと推定される。このようにSF。Figure 3 shows a typical parallel plate type reactive ion etching device using SF6 at 40 scem and etching pressure at 0.
.. The resist film and silicon oxide film (plasma CVD-3i02
This figure shows the hydrogenation dependence of the etching rate when etching a film. As is clear from this figure 3,
Addition of hydrogen increases the etching rate of both the resist film and the silicon oxide film. This is because when SFb is used alone, S generated from its discharge accumulates on the surface and suppresses etching, but when hydrogen is added, hydrogen radicals react with S to generate hydrogen sulfide (H2S), causing S It is presumed that this is to remove the SF like this.
に水素を添加した混合ガスは、レジスト膜及び酸化シリ
コン膜ともエツチング速度が増大し、エッチング速度が
等しい水素添加範囲を拡大できるため、該混合ガスによ
り前記レジスト膜から酸化シリコン膜の表層に亘ってエ
ッチバックすることにより、前述した酸素添加の場合と
同様、エツチング途中での酸素の発生に伴ってそれら膜
間のエツチングバランスが悪化することなく酸化シリコ
ン膜の表面を平坦化できる。A mixed gas in which hydrogen is added increases the etching rate of both the resist film and the silicon oxide film, and the range of hydrogen addition where the etching rate is equal can be expanded. By etching back, the surface of the silicon oxide film can be flattened without deteriorating the etching balance between the films due to the generation of oxygen during etching, as in the case of oxygen addition described above.
なお、上述したエッチバック効果は絶縁膜として酸化シ
リコンに代えてPSG等のガラスを用いた場合、有機高
分子材料膜としてレジストの代わりにポリイミドやポリ
スチレンを用いた場合にも同様に達成できる。Note that the above-mentioned etchback effect can be similarly achieved when a glass such as PSG is used instead of silicon oxide as the insulating film, and when polyimide or polystyrene is used instead of resist as the organic polymer material film.
(実施例)
以下、本発明の実施例を前述した第1図(A)〜(C)
を参照して詳細に説明する。(Example) The following is an example of the present invention shown in FIGS. 1 (A) to (C).
This will be explained in detail with reference to .
実施例1
まず、予め素子が形成された半導体基板1上にSiH4
及びN20のガスを用いるプラズマCVD法によりSi
O2からなる第1の層間絶縁膜2を堆積した後、A47
層の蒸着、パターニングにより第1層A、Q配線3を形
成した。つづいて、全面に第2の層間絶縁膜4を堆積し
た(第1図(A)図示)。Example 1 First, SiH4 was deposited on a semiconductor substrate 1 on which elements were formed in advance.
and Si by plasma CVD using N20 gas.
After depositing the first interlayer insulating film 2 made of O2, A47
The first layer A, Q wiring 3 was formed by layer deposition and patterning. Subsequently, a second interlayer insulating film 4 was deposited on the entire surface (as shown in FIG. 1(A)).
次いで、同図(B)に示すように第1層A、Q配線3を
含む第1の層間絶縁膜2上にSiH4及びN20のガス
を用いるプラズマCVD法により5in2からなる第2
の層間絶縁膜4を堆積した後、ポジ型フォトレジスを塗
布、乾燥して表面が平坦なレジスト膜5を形成した。Next, as shown in the figure (B), a second layer of 5in2 is formed on the first interlayer insulating film 2 including the first layer A and Q wiring 3 by a plasma CVD method using SiH4 and N20 gases.
After depositing the interlayer insulating film 4, a positive photoresist was applied and dried to form a resist film 5 with a flat surface.
次いで、前記半導体基板1を平行平板型反応性イオンエ
ツチング装置に設置し、SF6を40secm。Next, the semiconductor substrate 1 was placed in a parallel plate type reactive ion etching apparatus, and SF6 was etched for 40 seconds.
0□を20secm、エツチング圧力を0.05tor
r、印加周波数をIW / c、2の条件で、前記レジ
スト膜5から前記第2の層間絶縁膜4の表層に亘ってド
ライエツチングしてエッチバックした。この時、エツチ
ングの進行に伴って同一平面内に露出するレジスト膜5
の面積が減少し、5i02からなる第2の層間絶縁膜4
の面積が増大して雰囲気中の0□ガス量が増加するが、
同図(C)に示すように第2の層間絶縁膜4の表面を平
坦化できた。この後、第2の層間絶縁膜5上に第2層A
I配線(図示せず)をA1層の蒸着、バターニングによ
り形成したが、第2の層間絶縁膜4表面の平坦化により
第2層AΩ配線の段切れを防止することができた。0□ 20sec, etching pressure 0.05tor
Dry etching was carried out to etch back from the resist film 5 to the surface layer of the second interlayer insulating film 4 under the following conditions: r, applied frequency IW/c, 2. At this time, as the etching progresses, the resist film 5 exposed in the same plane
The area of the second interlayer insulating film 4 made of 5i02 is reduced.
The area of will increase and the amount of 0□ gas in the atmosphere will increase, but
As shown in FIG. 4C, the surface of the second interlayer insulating film 4 could be flattened. After this, a second layer A is formed on the second interlayer insulating film 5.
Although the I wiring (not shown) was formed by vapor deposition and buttering of the A1 layer, it was possible to prevent the second layer AΩ wiring from breaking by flattening the surface of the second interlayer insulating film 4.
実施例2
実施例1と同様なレジスト膜を被覆した半導体基板を、
平行平板型反応性イオンエツチング装置に設置し、SF
6を40scem、 H2を80secm、エツチング
圧力をQ、05tOrr、印加周波数をIW/Cl11
2の条件で、レジスト膜から第2の層間絶縁膜の表層に
亘ってドライエツチングしてエッチバックしたところ、
実施例1と同様に第2の層間絶縁膜の表面を平坦化する
ことができた。Example 2 A semiconductor substrate coated with a resist film similar to that of Example 1 was
Installed in parallel plate type reactive ion etching equipment, SF
6 to 40scem, H2 to 80sec, etching pressure to Q, 05tOrr, applied frequency to IW/Cl11
When dry etching was performed and etched back from the resist film to the surface layer of the second interlayer insulating film under the conditions of 2,
As in Example 1, the surface of the second interlayer insulating film could be flattened.
C発明の効果コ
以上詳述した如く、本発明のエッチバック方法によれば
エツチング中に同一平面内に露出した有機高分子材料膜
と酸化シリコン又はガラスからなる絶縁膜の面積が変化
してもそれらをほぼ等しい速度でエツチングして、前記
絶縁膜表面を良好に平坦化でき、ひいては゛)4導体装
置の多層配線工程に適用することによって段切れのない
信頼性の高い配線を形成できる等顕著な効果を奏する。C. Effects of the Invention As detailed above, according to the etchback method of the present invention, even if the areas of the organic polymer material film and the insulating film made of silicon oxide or glass exposed in the same plane during etching change, By etching them at approximately the same speed, the surface of the insulating film can be flattened well, and by applying it to the multilayer wiring process of a 4-conductor device, it is possible to form uninterrupted and highly reliable wiring. It has a remarkable effect.
第1図(A)〜(C)は多層配線構造を有する半導体集
積回路の標苧的な製造工程を示す断面図、第2図はSF
、と酸素の混合ガスによりレジスト膜と酸化シリコン膜
をエツチングした場合におけるそれら膜のエツチング速
度の酸素添加依存性を示す特性図、第3図はSF6と水
素の混合ガスによりレジスト膜と酸化シリコン膜をエツ
チングした場合におけるそれら膜のエツチング速度の水
素添加依存性を示す特性図、第4図はCF4と酸素の混
合ガスによりレジスト膜と酸化シリコン膜をエツチング
した場合におけるそれら膜のエツチング速度の酸素添加
依存性を示す特性図である。
■・・・半導体基板、2・・・第1の層間絶縁膜、3・
・・第1層、61配線、4・・・第2の層間絶縁膜、訃
・・レジスト膜。Figures 1 (A) to (C) are cross-sectional views showing the typical manufacturing process of a semiconductor integrated circuit having a multilayer wiring structure, and Figure 2 is an SF
A characteristic diagram showing the dependence of the etching rate of a resist film and a silicon oxide film on oxygen addition when a resist film and a silicon oxide film are etched with a mixed gas of SF6 and hydrogen. Figure 4 shows the dependence of the etching rate of these films on hydrogen addition when etching a resist film and a silicon oxide film with a mixed gas of CF4 and oxygen. It is a characteristic diagram showing dependence. ■... Semiconductor substrate, 2... First interlayer insulating film, 3...
...First layer, 61 wiring, 4...Second interlayer insulating film, and...Resist film.
Claims (1)
ラスからなる絶縁膜を形成し、この絶縁膜上に有機高分
子材料膜をその表面が平坦になるように被覆した後、前
記有機高分子材料膜から前記絶縁膜の表層に亘ってドラ
イエッチングしてエッチバックする方法において、前記
ドラエッチングをSF_6を主エッチングガスとし、こ
れに水素又は酸素を添加した混合ガスを用いて行うこと
を特徴とするエッチバック方法。An insulating film made of silicon oxide or glass having an uneven surface is formed on a semiconductor substrate, and an organic polymer material film is coated on this insulating film so that the surface is flat. In the method of performing dry etching and etching back over the surface layer of the insulating film, the dry etching is performed using SF_6 as the main etching gas and a mixed gas to which hydrogen or oxygen is added. Back method.