JPH03181585A - Polishing and grinding material - Google Patents

Polishing and grinding material

Info

Publication number
JPH03181585A
JPH03181585A JP32221689A JP32221689A JPH03181585A JP H03181585 A JPH03181585 A JP H03181585A JP 32221689 A JP32221689 A JP 32221689A JP 32221689 A JP32221689 A JP 32221689A JP H03181585 A JPH03181585 A JP H03181585A
Authority
JP
Japan
Prior art keywords
fiber
fibers
resin
hardness
abrasive
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP32221689A
Other languages
Japanese (ja)
Other versions
JP2830232B2 (en
Inventor
Masaji Harakawa
原川 正司
Shunji Uchio
舜二 内尾
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sumitomo Chemical Co Ltd
Original Assignee
Sumitomo Chemical Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sumitomo Chemical Co Ltd filed Critical Sumitomo Chemical Co Ltd
Priority to JP32221689A priority Critical patent/JP2830232B2/en
Publication of JPH03181585A publication Critical patent/JPH03181585A/en
Application granted granted Critical
Publication of JP2830232B2 publication Critical patent/JP2830232B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

PURPOSE:To obtain the title material capable of providing polished and ground face having higher precision, having high strength by itself, hardly damaged and also having excellent endurance by binding plural fibers having different hardness with a resin. CONSTITUTION:The aimed material obtained by binding (A) fiber [most preferably, alumina based fiber having >=60wt.% Al2O3 content and <=30wt.% SiO2 content, substantially free from alpha-Al2O3] consisting of alumina based fiber, silicon carbide fiber, silicon nitride fiber, etc. and having >=90kg/mm<2> (especially preferably >=120kg/mm<2>) Vickers hardness and (B) fiber consisting of a synthetic fiber such as rayon based fiber or polyester fiber and natural fiber and having low hardness with a resin, preferably epoxy resin, phenol resin, unsaturated polyester resin, polyimide resin, etc.

Description

【発明の詳細な説明】 〈産業上の利用分野〉 本発明は研磨研削材料に関する。[Detailed description of the invention] <Industrial application field> FIELD OF THE INVENTION This invention relates to abrasive grinding materials.

更に詳細には金属、セラs7クス、ガラス、樹脂、ゴム
、複合材料等を研磨研削する材料に関する。
More specifically, the present invention relates to materials for polishing and grinding metals, ceramics, glass, resins, rubber, composite materials, and the like.

〈従来技術〉 従来からの研磨研削材料は、ダイアモンド、ザクロ石、
ケイ砂等の天然研磨砥粒や熔融アルミナ、酸化ジルコニ
ウム、酸化チタン、炭化珪素、窒化珪素、窒化ボロン、
坑底アルミナ等の人工砥粒を鋳鉄等の金属や紙、布、不
織布等に塗布したり、樹脂や金属等で接着、または固め
た物が用いられてきた。
<Prior art> Traditional abrasive grinding materials include diamond, garnet,
Natural abrasive grains such as silica sand, fused alumina, zirconium oxide, titanium oxide, silicon carbide, silicon nitride, boron nitride,
Artificial abrasive grains such as bottom alumina have been applied to metals such as cast iron, paper, cloth, non-woven fabrics, etc., or bonded or hardened with resins, metals, etc. have been used.

さらには、これら砥粒に、高強度の繊維を補強材として
樹脂で固めた砥石が、特開昭52−3796号公報、特
開昭54−82786号公報、特開昭55−13147
3号公報、特開昭59−97845号公報、特開昭63
−34072号公報などに提案されている。
Furthermore, whetstones in which these abrasive grains are hardened with resin using high-strength fiber as a reinforcing material are disclosed in JP-A-52-3796, JP-A-54-82786, and JP-A-55-13147.
Publication No. 3, JP-A-59-97845, JP-A-63
This is proposed in, for example, Publication No.-34072.

コノ他、USP−3972161号公報には、砥粒に代
えてモース硬度9.3〜9.6のボロン繊維を樹脂で固
めた砥石が開示されている。
US Pat. No. 3,972,161 by Kono et al. discloses a grindstone in which boron fibers having a Mohs hardness of 9.3 to 9.6 are hardened with a resin instead of abrasive grains.

これら研磨研削材料において、被研磨研削物の屑排出不
良により生ずる種々の障害例えば、研磨研削材料の目詰
りによる効率の低下、屑による加工面の損傷などの防止
の為研磨研削材料中に空孔を設けることが行われている
。
In these abrasive and abrasive materials, holes are formed in the abrasive and abrasive material in order to prevent various problems caused by poor evacuation of debris from the material to be polished. is being established.

〈発明が解決しようとする課題〉 研磨研削材料に空孔を設けた研磨材料は、空孔に相当す
る分だけ砥粒の含有率が低下し研磨研削性能や耐久性が
劣り、しかも研磨研削材自身の強度も低下するので研磨
精度が悪くなったり、耐久性が低下し、加工途中で損傷
したりするので寿命が短くなるという欠点が有る。
<Problem to be solved by the invention> In an abrasive material in which pores are provided, the abrasive grain content decreases by the amount corresponding to the pores, resulting in poor abrasive grinding performance and durability. Since the strength of the material itself decreases, the polishing accuracy deteriorates, the durability decreases, and it can be damaged during processing, resulting in a shortened service life.

又、研磨研削作業において潤滑や冷却の目的で、水や油
や各種液体を用いることが有るが樹脂や金属で固めた研
磨研削材においては、緻密な構造のため水や油が含浸さ
れにいので研磨研削作業で摩擦が大きくなり作業性が悪
い上、被研磨研削物の加工面の精度がでにくいなどの問
題を有する。
In addition, water, oil, and various other liquids are sometimes used for lubrication and cooling purposes in abrasive grinding work, but abrasive materials hardened with resin or metal have a dense structure that prevents them from being impregnated with water or oil. Therefore, there are problems such as increased friction during abrasive grinding work, resulting in poor workability, and difficulty in achieving precision on the machined surface of the object to be polished.

く課題を解決するための手段〉 本発明は、硬度の異なる二種以上の繊維を樹脂で結合し
てなる研磨研削材料を提供するものである。
Means for Solving the Problems> The present invention provides an abrasive grinding material made by bonding two or more types of fibers with different hardnesses with a resin.

本発明にいう研磨研削材料とは、各種材料を研磨研削す
るのに供されるものをいう。
The term "abrasive grinding material" as used in the present invention refers to a material used for abrasive grinding of various materials.

本発明で用いられる繊維は、硬度の異なる二種以上の繊
維による種々の組合せがある。
The fibers used in the present invention include various combinations of two or more types of fibers having different hardnesses.

硬度の高い繊維としては、ビッカース硬度で90Kg/
mm”、好ましくは100Kg/−7以上より好ましく
は120Kg/mm”以上の周知の金属繊維やセラミッ
クス繊維が適している。
As a fiber with high hardness, Vickers hardness is 90kg/
Well-known metal fibers and ceramic fibers having a diameter of 100 Kg/mm", preferably 100 Kg/-7 or more, more preferably 120 Kg/mm" or more are suitable.

具体的には、アル鋭す質繊維、シリカ繊維、炭化珪素繊
維、チラノ繊維、窒化珪素繊維、ガラス繊維、シリコン
オキシナイトライド繊維、等のセラミック繊維;スチー
ル繊維、ステンレス繊維、ボロン繊維、タングステン繊
維等の金属繊維:炭素繊維が該当する。
Specifically, ceramic fibers such as aluminum sharp fibers, silica fibers, silicon carbide fibers, tyranno fibers, silicon nitride fibers, glass fibers, silicon oxynitride fibers; steel fibers, stainless steel fibers, boron fibers, tungsten fibers Metal fibers such as carbon fibers are applicable.

なかでもアルミナ質繊維、炭化珪素繊維、窒化珪素繊維
は、硬度が高い上に高強度で耐熱性、耐食性に優れるの
で好適である。
Among these, alumina fibers, silicon carbide fibers, and silicon nitride fibers are preferred because they have high hardness, high strength, and excellent heat resistance and corrosion resistance.

特に、A1.03が60重量%以上、Sif!が30重
量%以下の成分からなりX線的構造においてα−^hO
tの反射を実質的に示さないアルミナ質繊維は高強度、
高弾性率でしかも高硬度であるのでとくに適している。
In particular, A1.03 is 60% by weight or more, Sif! consists of 30% by weight or less, and the X-ray structure shows α-^hO
Alumina fibers with virtually no reflection of t have high strength;
It is particularly suitable because it has a high modulus of elasticity and high hardness.

これらの硬度の高い繊維は、硬度のほか、強度、耐衝撃
性、熱伝導率等の物性のバランスをとるため2種以上を
組合せても良い。
Two or more of these highly hard fibers may be used in combination in order to balance physical properties such as strength, impact resistance, and thermal conductivity in addition to hardness.

硬度の高い繊維の形状としては、まずその長さは、研磨
研削性能から、および研磨研削材料自体の機械的強度の
補強効果から10mm以上、好ましくは15問以上、よ
り好ましくは20開以上の長さをか好ましい。
Regarding the shape of the fibers with high hardness, first, the length should be 10 mm or more, preferably 15 mm or more, more preferably 20 mm or more, from the viewpoint of abrasive grinding performance and the reinforcing effect on the mechanical strength of the abrasive material itself. I like it.

該研磨研削材料中の硬度の高い繊維の含有率を高くする
には、連続長繊維が適している。
Continuous long fibers are suitable for increasing the content of hard fibers in the abrasive material.

連続長繊維の場合は、ストランド、ヤーン、布、紐等の
形状で用いる。
In the case of continuous filaments, they are used in the form of strands, yarns, cloth, strings, etc.

次に、硬度の高い繊維の太さについては、太い程研磨研
削効率は優れるが研磨研削面の平滑性や精度は劣り、細
い程研磨研削面の平滑性は優れるが効率が劣るので、繊
維の直径は、3μ〜150μ程度でそれぞれの用途に応
して適宜選択すれば良い。
Next, regarding the thickness of the fibers with high hardness, the thicker the abrasive grinding efficiency, but the smoothness and precision of the abrasive grinding surface is inferior, and the thinner the abrasive grinding surface, the smoothness is better but the efficiency is lower. The diameter may be appropriately selected from about 3 μm to 150 μm depending on each application.

従って、太さのばらつきは、研磨研削精度を低下させる
ので、小さい程望ましい。
Therefore, it is desirable that the variation in thickness be as small as possible since it reduces the precision of polishing and grinding.

硬度の低い繊維としてはレーヨン系繊維、ポリアミド繊
維、ポリエステル繊維、アクリル繊維7ビニロン繊維2
ポリエチレン繊維、ポリプロピレン繊維、塩化ビニール
繊維、テフロン繊維等の合成繊維;木綿、麻、羊毛、絹
、こうぞ、三唖、ジュート等の天然繊維が主として用い
られる。
Fibers with low hardness include rayon fiber, polyamide fiber, polyester fiber, acrylic fiber 7 vinylon fiber 2
Synthetic fibers such as polyethylene fibers, polypropylene fibers, vinyl chloride fibers, and Teflon fibers; natural fibers such as cotton, hemp, wool, silk, kozo, mitten, and jute are mainly used.

これらの繊維も複数の種類を用いてよい。Plural types of these fibers may also be used.

該硬度の低い繊維は、長フィラメントや紡糸による連続
長繊維のストランド、ヤーン、紐、織布、不織布の形態
、短繊維のまま等の形態でも用いることが出来る。
The low-hardness fibers can be used in the form of long filaments, continuous long fiber strands, yarns, strings, woven fabrics, non-woven fabrics, or as short fibers.

硬質の高い繊維と硬度の低い繊維の比率は、硬質の高い
繊維の割合が高い程、削る性能が優れるので用途及び使
用条件に合わせて20容量%から80容量%の範囲で選
択する。
The ratio of fibers with high hardness to fibers with low hardness is selected in the range of 20% by volume to 80% by volume depending on the purpose and conditions of use, since the higher the ratio of fibers with higher hardness is, the better the cutting performance is.

好ましくは、硬質の高い繊維の割合が50〜90容量%
である。
Preferably, the proportion of highly rigid fibers is 50 to 90% by volume.
It is.

二種類以上の繊維を結合する樹脂としては、エポキシ樹
脂、フェノール樹脂、不飽和ポリエステル樹脂、ビニル
エステル樹脂、アルキッド樹脂、尿素−ホルマリン樹脂
、ポリイミド樹脂等の熱硬化性樹脂;ポリエチレン、ポ
リプロピレン、ポリメチルメタクリレート、ポリスチレ
ン、ポリ塩化ビニール、ABS樹脂、AS樹脂、ポリア
ミド、ポリアセタール、ポリスルフォン、ポリカーボネ
ート、ポリフェニレンオキサイド、、HIJエーテルス
ルフォン、ポリエーテルエーテルケトン、ポリアミトイ
ミド、ポリウレタン等の熱可塑性樹脂がある。
Examples of resins that bind two or more types of fibers include thermosetting resins such as epoxy resins, phenolic resins, unsaturated polyester resins, vinyl ester resins, alkyd resins, urea-formalin resins, and polyimide resins; polyethylene, polypropylene, and polymethyl There are thermoplastic resins such as methacrylate, polystyrene, polyvinyl chloride, ABS resin, AS resin, polyamide, polyacetal, polysulfone, polycarbonate, polyphenylene oxide, HIJ ether sulfone, polyether ether ketone, polyamitimide, and polyurethane.

これらの中でエポキシ樹脂、フェノール樹脂、不飽和ポ
リエステル樹脂、ボリイくド樹脂等の樹脂が特に好適で
ある。
Among these, resins such as epoxy resins, phenol resins, unsaturated polyester resins, and solid resins are particularly suitable.

これらの樹脂による硬度の異なる二種以上の繊維の結合
の形態については、二種以上の繊維が近接して存在すれ
ば如何なる形態でも良い。
The form of bonding of two or more types of fibers having different hardness by these resins may be any form as long as the two or more types of fibers are present in close proximity.

例えば、これらの繊維が、連続長繊維であれば、単繊維
またはヤーン単位で混合あるいは混繊したもの、一方向
に揃えて積層した状態で結合したもの、布状のものは積
層して結合したもの、短繊維は単に混合して結合したも
の、長繊維に短繊維をほぼ均一に分散させて結合したも
のがあげられる。
For example, if these fibers are continuous filaments, they may be mixed or mixed as single fibers or yarns, they may be aligned in one direction and bonded in a laminated state, or cloth-like fibers may be laminated and bonded. Short fibers may be simply mixed and bonded, or short fibers may be bonded by substantially uniformly dispersing short fibers into long fibers.

尚、硬度の高い繊維成分と硬度の低い繊維成分とが芯−
鞘構造になっている繊維を集合して結合したものも該当
する。
In addition, the fiber component with high hardness and the fiber component with low hardness are the core.
This also applies to fibers that are assembled and bonded to form a sheath structure.

樹脂による硬度の異なる二種以上の繊維を結合するには
、繊維強化複合材料を作る周知の方法が適用できる。
In order to combine two or more types of fibers with different hardnesses using resin, a well-known method for producing a fiber reinforced composite material can be applied.

つまり、熱硬化性樹脂では、未硬化又は半硬化あるいは
溶剤に溶かした状態で、熱可塑性樹脂では、溶融又は溶
剤に溶かした状態で、連続長繊維や布状のものに含浸さ
せる所謂プリプレグの製造方法が適用できる。
In other words, thermosetting resins are uncured or semi-cured or dissolved in a solvent, and thermoplastic resins are molten or dissolved in a solvent and impregnated into continuous filaments or cloth to produce so-called prepreg. method can be applied.

繊維の形状が短繊維の場合は、そのまま樹脂に混合して
もよいが、一般にシートモールデイングコンパウンドと
称される方法(以下SMC法と称す)が適用できる。
If the fibers are short fibers, they may be mixed directly into the resin, but a method generally called sheet molding compound (hereinafter referred to as SMC method) can be applied.

SMC法によれば、一方が短繊維で他方が長繊維を揃え
たものや布状のものにも適用できる。
According to the SMC method, it can be applied to materials in which short fibers are arranged on one side and long fibers on the other, or cloth-like materials.

繊維を樹脂で固めたものを、種々の研磨研削材料の形状
に成形する方法は、繊維強化複合材料で用いられている
各種の成形方法が採用できる。
Various molding methods used for fiber-reinforced composite materials can be used to mold fibers hardened with resin into the shapes of various abrasive materials.

短繊維をそのまま樹脂に混合したものは、射出成形等が
用いられる。
Injection molding or the like is used to mix short fibers directly into resin.

連続長繊維の場合は、プリプレグ11層法、フィラメン
トワインディング法、プルトルージョン法等がある。
In the case of continuous filaments, methods include the 11-layer prepreg method, the filament winding method, and the pultrusion method.

尚、硬度の高い繊維と硬度の低い繊維とを別々に樹脂で
固めたものをこの成形の際に積層したり、一方の繊維を
樹脂で固めたシートを重ねその間に他方の繊維を挟み込
み成形することにより、成形の際に2種以上の繊維を組
合わすこともできる。
In addition, fibers with high hardness and fibers with low hardness that are hardened separately with resin are laminated during this molding, or sheets of one fiber hardened with resin are stacked and the other fiber is sandwiched between them and molded. Accordingly, two or more types of fibers can be combined during molding.

これらの方法により、研磨研削材料の形状は板、棒、パ
イプ、円盤等使途に合わせて任意の物を用いることが出
来る。
By these methods, the shape of the abrasive material can be any shape, such as a plate, rod, pipe, disk, etc., depending on the intended use.

また、高強度、高剛性を遠戚するためには応力の方向に
繊維が配向するよう成形体の形状を定めればよい。
Further, in order to achieve high strength and high rigidity, the shape of the molded body may be determined so that the fibers are oriented in the direction of stress.

なお、研磨研削材料のなかに含まれる全繊維の量は、6
0〜90容積%の範囲で適宜選べば良い。
The total amount of fibers contained in the abrasive material is 6
It may be appropriately selected within the range of 0 to 90% by volume.

この量の調節も、繊維強化複合材料を作る周知の方法が
適用できる。
A well-known method for producing fiber-reinforced composite materials can also be applied to adjust this amount.

(発明の効果〉 本発明の研磨研削材は、含水含油性を有し摩擦抵抗が少
ないので低動力で研磨研削できる。
(Effects of the Invention) The abrasive material of the present invention has water- and oil-retaining properties and low frictional resistance, so that it can be abrasively ground with low power.

本発明の研磨研削材料は、硬度の低い繊維を併用するこ
とにより研磨研削の際に、余分な応力が掛かっても、そ
れが吸収出来るためか、より精度の高い研磨研削面が達
成され上、研磨研削材料自体が高強度で損傷しに<<、
耐久性にも優れる。
The abrasive grinding material of the present invention is able to absorb extra stress during abrasive grinding by using fibers with low hardness, and a more precise abrasive surface is achieved. The abrasive grinding material itself has high strength and will not be damaged.
It also has excellent durability.

〈実施例〉 以下実施例にて更に説明するが本発明はこれに限定され
るものではない。
<Example> The present invention will be further described below with reference to Examples, but the present invention is not limited thereto.

実施例1 スミ◇エポキシELA−134(、ビスフェノ−a A
型工fキシ樹脂住友化学工業■製)60wt%とスミ■
エポキシESCN −220H(クレリールノネラフク
型工lキシ樹脂住友化学業■製)製)40wt%にジシ
アンジアミド5部、  3−(3,4ンクロロフエニル
)−1,1−ンメチル尿素 4wt  %を混合し75
℃に加熱し、これを連続した離型紙上に流下しドクター
ナイフを通過して樹脂膜を得た。
Example 1 Sumi◇Epoxy ELA-134 (, Bispheno-a A
Moldwork f xy resin manufactured by Sumitomo Chemical Co., Ltd.) 60wt% and Sumitomo ■
5 parts of dicyandiamide and 4 wt % of 3-(3,4-chlorophenyl)-1,1-methylurea were mixed with 40 wt% of epoxy ESCN-220H (manufactured by Sumitomo Chemical Co., Ltd.). 75
The mixture was heated to .degree. C., poured down onto a continuous release paper, and passed through a doctor knife to obtain a resin film.

アルミナ繊維Altex  (住友化学製AlzOゴ8
5%、 5iOil 5%)を一方向に引き揃えシート
状に広げた。これにレーヨン繊維の織布(旭化戒工業陣
製)を重ねてから樹脂膜が塗られた離型紙を上下から挟
み120℃のプレスロールに3Kg/cmの線圧をかけ
て、アルミナ繊維70容積%、レーヨン繊維30容積%
の比率で繊維目付け330g/m”のプリプレグを得た
。
Alumina fiber Altex (Sumitomo Chemical AlzO Go8
5% and 5iOil 5%) were aligned in one direction and spread out into a sheet shape. A rayon fiber woven fabric (manufactured by Asahi Kakai Kogyo Jin) was layered on top of this, release paper coated with a resin film was sandwiched from above and below, and a linear pressure of 3 kg/cm was applied to a press roll at 120°C. Volume%, rayon fiber 30% by volume
A prepreg with a fiber basis weight of 330 g/m'' was obtained at this ratio.

このプリプレグを30cmの正方形に切り出し42枚積
層した後、金型に入れ5Kg/cm” 、  120℃
でホットプレスし硬化板を得た。
After cutting out this prepreg into 30cm squares and laminating 42 sheets, they were put into a mold and heated to 5Kg/cm" at 120℃.
A hardened plate was obtained by hot pressing.

これをダイアモンドカッターで幅10問厚みII長さ5
01111に切り出し、超音波研磨機(スタンレー電気
製)に取り付はプレハードンw4製の29インチのテレ
ビキャビネット用射出戒型金型を研磨した。
Use a diamond cutter to cut this into 10 widths, thickness II, and 5 lengths.
01111, and attached to an ultrasonic polisher (manufactured by Stanley Electric) to polish a pre-hardened W4 injection mold for a 29-inch television cabinet.

研磨精度が飽和するまでの所要時間、研磨精度を測定し
た。
The time required for polishing accuracy to reach saturation and polishing accuracy were measured.

また、該材料を連続して使用可能な時間を測定した。 
 結果を表1に示す。
In addition, the time during which the material could be used continuously was measured.
The results are shown in Table 1.

実施例2〜4 アルミナ繊維としてA I texに代えてFP(Du
Pont製)、Alcen(11気化学工業■製)、N
exte1312 (3M社製)を用いた以外は実施例
1と同様に行った。
Examples 2 to 4 FP (Du
(manufactured by Pont), Alcen (manufactured by 11 Ki Kagaku Kogyo ■), N
The same procedure as in Example 1 was conducted except that exte1312 (manufactured by 3M) was used.

結果を表1に示す。The results are shown in Table 1.

表1 実施例5 アルミナ繊維Altexの平織り織物(日付け630 
g /msりに、予め1〜5IIffiの長さのアクリ
ル繊維を15%混合したスミ■エポキシELA −12
8(ビアフェノールA型エポキシ樹脂住友化学工業■製
)、ジシアンジアミド(日本触媒化学社製)、叶バーF
+−95(DuPon を社製)を含浸させアルミナ繊
維75容積%、アクリル繊維25容積%の繊維比率を有
するプリプレグを得た。
Table 1 Example 5 Plain weave fabric of alumina fiber Altex (date 630
g/ms, Sumi Epoxy ELA-12 is pre-mixed with 15% of acrylic fibers with a length of 1 to 5Iffi.
8 (Biaphenol A type epoxy resin manufactured by Sumitomo Chemical Co., Ltd.), dicyandiamide (manufactured by Nippon Shokubai Kagaku Co., Ltd.), Kano Bar F
+-95 (manufactured by DuPon) to obtain a prepreg having a fiber ratio of 75% by volume of alumina fibers and 25% by volume of acrylic fibers.

このプリプレグから、中心に151111の穴を打ち抜
いた直径1001I11の円形のシートを切り出した。
A circular sheet with a diameter of 1001I11 was cut out from this prepreg with a hole of 151111 punched in the center.

このシートを10枚重ねたドーナツ状の積層体をオフセ
ット型に入れ、5Kg/cm” 、180℃で2時間ホ
ットプレスし全繊維が60容積%の円盤状の研削材が得
られた。
A donut-shaped laminate of 10 of these sheets was placed in an offset mold and hot pressed at 5 kg/cm'' at 180° C. for 2 hours to obtain a disc-shaped abrasive material containing 60% by volume of total fibers.

これを日立製作所型の100φオフセ−/ )グライン
ダーの取り付け1200rpmで厚み10叩のアルミニ
ウムを研削した。
This was attached to a Hitachi model 100φ offset grinder at 1200 rpm to grind aluminum with a thickness of 10 strokes.

研削速度の低下も無く端正な切口を保持したまま100
000■研削した。
100 without reducing the grinding speed and maintaining a neat cut
000■Grinded.

切口の端面ば平滑で鏡面に仕上がっていた。The cut edges were smooth and had a mirror finish.

実施例6 一方向引き揃えたアルミナ繊維A l texにスミ■
エポキシELM−434(ビスフェノールA型xiキシ
樹脂住友化学工業■製)、ジンアンジアミド(日本触媒
化学社製) 、スミキュアーS (ジアミノジフェニル
スル7オン住友化学工業■製)の混合物を含浸させプリ
プレグ(目付け150g/ms”)を得た。
Example 6 Ink on alumina fiber A l tex aligned in one direction
Prepreg ( A basis weight of 150 g/ms") was obtained.

このプリプレグにポリプロピレン繊維の不織布を重ね合
わせ、内径5門のマンドレルにアルミナ繊維が±45°
の角度に配向するように順次巻き付は外径10+amま
で積層し、さらにその外側を3Kgの張力でポリエステ
ル製のテープを巻いた後、120℃で2時間加熱硬化し
、繊維含有率85容積%(内アルミナ繊維を55容積%
)含むパイプを作製した。
This prepreg is overlaid with a non-woven fabric made of polypropylene fibers, and alumina fibers are placed on a mandrel with an inner diameter of ±45°.
The layers were sequentially wrapped so that they were oriented at an angle of 10+am, and then a polyester tape was wrapped around the outside with a tension of 3 kg, and then heated and cured at 120°C for 2 hours, with a fiber content of 85% by volume. (55 volume% inner alumina fiber
) was produced.

このバイブ5本をターンテーブルに固定し、周速が12
2ffi/分で回転させなから150φのアルミニウム
板を研磨した所、0.07μの仕上げ面が得られた。
These five vibrators are fixed to a turntable, and the circumferential speed is 12
When a 150φ aluminum plate was polished while rotating at 2ffi/min, a finished surface of 0.07μ was obtained.

比較例1〜4 レーヨン繊維を除いた以外は実施例1〜4と同様に行っ
た。
Comparative Examples 1-4 Comparative Examples 1-4 were carried out in the same manner as Examples 1-4 except that the rayon fiber was removed.

結果を表2に示す。The results are shown in Table 2.

表 2 比較例5 アクリル繊維を除いた以外は実施例6と同様に行った。table 2 Comparative example 5 The same procedure as in Example 6 was conducted except that the acrylic fibers were removed.

研磨面は、目視でも凸凹の筋が認められ程不良であった
。
The polished surface was so poor that uneven streaks were visible even when visually observed.

Claims (1)

【特許請求の範囲】[Claims] 硬度の異なる二種以上の繊維を樹脂で結合してなる研磨
研削材料。
An abrasive material made by bonding two or more types of fibers with different hardness with resin.
JP32221689A 1989-12-11 1989-12-11 Abrasive grinding material Expired - Fee Related JP2830232B2 (en)