JPH03187942A - Production of polarization maintaining optical fiber - Google Patents

Production of polarization maintaining optical fiber

Info

Publication number
JPH03187942A
JPH03187942A JP1327039A JP32703989A JPH03187942A JP H03187942 A JPH03187942 A JP H03187942A JP 1327039 A JP1327039 A JP 1327039A JP 32703989 A JP32703989 A JP 32703989A JP H03187942 A JPH03187942 A JP H03187942A
Authority
JP
Japan
Prior art keywords
sio
layer
core rod
optical fiber
core
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
JP1327039A
Other languages
Japanese (ja)
Inventor
Masahiro Takagi
政浩 高城
Hiroshi Suganuma
寛 菅沼
Hiroshi Yokota
弘 横田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sumitomo Electric Industries Ltd
Original Assignee
Sumitomo Electric Industries Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sumitomo Electric Industries Ltd filed Critical Sumitomo Electric Industries Ltd
Priority to JP1327039A priority Critical patent/JPH03187942A/en
Publication of JPH03187942A publication Critical patent/JPH03187942A/en
Ceased legal-status Critical Current

Abstract

PURPOSE:To produce a polarization maintaining optical fiber having excellent transmission characteristics, etc., in high yield by grinding a core rod composed of a core part and a clad part to elliptic cross-section, successively forming a stress-imparting layer and a jacket layer on the outer circumference and spinning the product. CONSTITUTION:A core rod 3 composed of a core part 1 having high refractive index and a clad part 2 having a refractive index lower than that of the core part 1 is prepared beforehand. The core rod 3 is ground to nearly elliptic cross- section. A glass soot layer 4 containing B and P is formed on the outer circumference of the processed core rod 3 by VAD process and the layer is sintered to form a stress-imparting layer 5 on the outer circumference of the core rod 3. Subsequently, the product is inserted and fixed into a glass tube made of a material same as the material of the clad 2 and the assembly is spun to obtain a polarization maintaining optical fiber having a jacket layer 6 formed on the outer circumference of the stress-imparting layer 5.

Description

【発明の詳細な説明】 (産業上の利用分野) 本発明は伝送特性のすぐれた偏波面保存光ファイバを歩
留りよく製造する偏波面保存光ファイバの製造方法に関
するものである。
DETAILED DESCRIPTION OF THE INVENTION (Industrial Field of Application) The present invention relates to a method for manufacturing a polarization-maintaining optical fiber with high yield, which produces a polarization-maintaining optical fiber with excellent transmission characteristics.

(従来の技術) 従来、楕円ジャケット型の偏波面保存光ファイバは、次
の■〜■の工程に従って製造されていた。
(Prior Art) Conventionally, an elliptical jacket type polarization maintaining optical fiber has been manufactured according to the following steps (1) to (2).

■GeドープSho□のコアとシリカクラッドとから成
るコアロッドを直径P2O5、SiOIll程度に延伸
する。
(2) A core rod consisting of a Ge-doped Sho□ core and a silica cladding is stretched to a diameter of approximately P2O5 and SiOIll.

■サポート管トナル直径16m1lP2O5、SiO肉
厚1.5mlP2O5、SiO程度の出発石英管内壁に
MCVD法によりB及びPを堆積させる。この堆積層が
楕円ジャケット部となる。
(2) Support tube diameter: 16 ml P2O5, SiO wall thickness: 1.5 ml P2O5, B and P are deposited on the inner wall of the starting quartz tube of approximately SiO by the MCVD method. This deposited layer becomes the elliptical jacket part.

■このサポート管↓減圧、加熱することにより楕円化し
た後、管内に■で延伸されたコアロッドをロッドインし
、カラブス及び真円化してファイバ母材とする。
■This support tube↓ is depressurized and heated to make it oval, and then the core rod drawn in ■ is inserted into the tube, and the support tube is made into a carabous and perfect circle to form a fiber base material.

■この光フアイバ母材を線引きして楕円ジャケット型偏
波面保存光ファイバを得る。
■This optical fiber base material is drawn to obtain an elliptical jacket type polarization maintaining optical fiber.

(解決しようとする課題) 上述した従来の製造方法においては、前記の■の工程に
よる楕円化において減圧値、加熱温度、サポート管の内
外径及びBとPのガラス膜圧や組成等の多種の要因に大
きく影響を受け、これらいずれかの値かわずかに変化し
ても楕円率が大きく異なってしまう。従って、楕円率の
再現性や長手方向の均一性に乏しく、このためクロスト
ーク特性が低下するという問題があった。このクロスト
ーク特性を改善する方法として楕円率を大きくし、かつ
Bのモル濃度を高く設定する方法があるが、Bのモル濃
度を高くすると粘性が低下するので楕円形状の均一化が
一層困難となってしまう。
(Problems to be Solved) In the conventional manufacturing method described above, various changes are made in the ovalization in the step It is greatly influenced by various factors, and even a slight change in any one of these values will result in a large difference in the ellipticity. Therefore, there is a problem in that the reproducibility of ellipticity and the uniformity in the longitudinal direction are poor, and therefore the crosstalk characteristics are deteriorated. One way to improve this crosstalk characteristic is to increase the ellipticity and set the molar concentration of B high, but increasing the molar concentration of B lowers the viscosity, making it even more difficult to make the elliptical shape uniform. turn into.

又コアロッド及び出発石英管のサイズを上述の値より大
きくしようとすると、コアロッドとサポート管との一体
化時にクラックが発生し易くなり、このため、例えばI
Okm以上の長尺化が困難となる。
Furthermore, if the size of the core rod and starting quartz tube is made larger than the above-mentioned values, cracks are likely to occur when the core rod and support tube are integrated, and for this reason, for example, if the size of the I
It becomes difficult to make the length longer than 0 km.

さらに、コアロッドをロッドインする際に、これらの中
心合せが難しく、ファイバの偏心が大きくなり易いとい
う問題もあった。
Furthermore, when inserting the core rod, it is difficult to center the core rod, and the eccentricity of the fiber tends to increase.

上述の問題点を解消する一手段として、例えば特開昭6
3−303823号に示されるような製造方法が提案さ
れている。この方法は、Ge含有コアとシリカクラッド
とから成るコアロッドを断面楕円形状に研削加工した後
、その外周部にB及びPを含有するガラス微粒子を外付
けして焼結、線引きするものである。
As a means of solving the above-mentioned problems, for example,
A manufacturing method as shown in No. 3-303823 has been proposed. In this method, a core rod consisting of a Ge-containing core and a silica cladding is ground into an elliptical cross-section, and then glass fine particles containing B and P are attached to the outer periphery of the core rod, followed by sintering and drawing.

しかし、この方法によれば前述の問題点の一部は解決可
能であるが、コアに複屈折性を与えるべき応力付与層の
周囲は自由表面であるため、コア、クラッドと応力付与
層の熱膨張の差に起因するコア、クラッド部分に加わる
応力が小さくなってしまい、充分満足のいく特性が得ら
れないという問題点がある。
However, although some of the above-mentioned problems can be solved by this method, since the area around the stress-applying layer that should impart birefringence to the core is a free surface, the heat of the core, cladding, and stress-applying layer increases. There is a problem in that the stress applied to the core and cladding portions due to the difference in expansion becomes small, making it impossible to obtain sufficiently satisfactory characteristics.

(課題を解決するための手段) 本発明は上述の問題点を解消し、伝送特性のすぐれた偏
波面保存光ファイバを歩留りよく製造する偏波面保存光
ファイバの製造方法を提供するもので、その特徴は、屈
折率の高いコア部と、該コア部の屈折率よりも屈折率の
低いクラッド部から成るコアロッドを、断面略楕円形状
に研削加工した後、その外周部に応力付与層及びジャケ
ット層を順次形成し、ついで紡糸することにある。
(Means for Solving the Problems) The present invention solves the above-mentioned problems and provides a method for manufacturing a polarization-maintaining optical fiber with excellent transmission characteristics at a high yield. The feature is that a core rod consisting of a core portion with a high refractive index and a cladding portion with a lower refractive index than the core portion is ground into a roughly elliptical cross section, and then a stress applying layer and a jacket layer are added to the outer periphery of the core rod. The process involves sequentially forming and then spinning.

(作用) 上述した本発明の製造方法においては、コアロッドを研
削加工して直接楕円形状となし、その外周部に応力付与
層及びジャケット層を順次形成して母材となし、これを
紡糸する。
(Function) In the manufacturing method of the present invention described above, a core rod is directly ground into an elliptical shape, a stress applying layer and a jacket layer are sequentially formed on the outer circumference of the core rod to form a base material, and this is spun.

上記応力付与層により異方性の応力を加えるものである
が、この際、応力付与層の外周部にはジャケット層が存
在するため充分満足のいくすぐれた特性が得られる。
Anisotropic stress is applied by the above-mentioned stress applying layer, and in this case, since a jacket layer is present on the outer periphery of the stress applying layer, sufficiently satisfactory and excellent characteristics can be obtained.

又コアロッドの楕円形状は容易に均一化がなされ、コア
ロッドを太くしてもクラックが発生することがな(、長
尺化が可能となる。
In addition, the elliptical shape of the core rod can be easily made uniform, and even if the core rod is made thicker, cracks will not occur (and the core rod can be made longer).

(実施例) 第1図(イ)〜(ネ)は本発明の偏波面保存光ファイバ
の製造方法の実施例に係る工程図である。
(Example) FIGS. 1A to 1E are process diagrams relating to an example of the method for manufacturing a polarization-maintaining optical fiber of the present invention.

第1図(イ)に示すように、比屈折率差0.4%のGe
l・−プSIOのコア(1)及びシリカクラッド(2)
からなる直径15In+1、長さ50cmのコアロッド
(3)を研削して、同図(ロ)のように、長軸径15■
鵬、短軸径7.5m+a(楕円率33%)の断面楕円形
状に加工する。なお、コア径は0.15mmである。
As shown in Figure 1 (a), Ge with a relative refractive index difference of 0.4%
l-P SIO core (1) and silica cladding (2)
A core rod (3) with a diameter of 15In+1 and a length of 50cm is ground to give a long axis diameter of 15mm as shown in the same figure (b).
Peng is processed into an elliptical cross-sectional shape with a minor axis diameter of 7.5 m+a (ellipticity 33%). Note that the core diameter is 0.15 mm.

次に、楕円加工されたコアロッド(3)の外周部に、同
図(ハ)のように、■AD法によりB及びPを含存する
ガラス微粒子層(4)をガラス微粒子生成用バーナ(4
I)により外付けする。このとき、焼結後の外径が20
m+nとなるようにガラス微粒子の外付けを行なう。又
Bのモル濃度は8mO!%程度とし、Pはこの外付は部
の屈折率がシリカと同じ値になるように設定してドープ
する。このようにして外付けされたコアロッド(3)を
焼結することにより、同図(ニ)に示すように、コアロ
ッド(3)の外周部に応力付与層(5)が形成された母
材を得る。
Next, as shown in FIG.
I). At this time, the outer diameter after sintering is 20
Glass particles are externally attached so that m+n. Also, the molar concentration of B is 8 mO! %, and P is set and doped so that the refractive index of this external part has the same value as silica. By sintering the externally attached core rod (3) in this way, a base material with a stress-applying layer (5) formed on the outer periphery of the core rod (3) is created, as shown in FIG. obtain.

次に」1記母材をあらかじめ成形したクラッド(2)と
同質の内径22mmφ、外径26.7mmφのガラス管
内に挿入固定してファイバ用母材を得、このファイバ母
材を紡糸して同図(ネ)のような応力付与層(5)の外
周部にジャケット層(6)を形成した偏波面保存光ファ
イバを製造する。
Next, the base material 1 is inserted and fixed into a glass tube with an inner diameter of 22 mmφ and an outer diameter of 26.7 mmφ, which is the same as the pre-formed cladding (2), to obtain a fiber base material, and this fiber base material is spun into the same material. A polarization-maintaining optical fiber in which a jacket layer (6) is formed on the outer periphery of a stress applying layer (5) as shown in Figure (N) is manufactured.

以上のようにして、条長10kmの偏波面保存光ファイ
バを製造し、評価したところ、その伝送損失は波長1.
55mmで0.22dB/km1モード複屈折率はe 
x to−’及び偏心度は0.1μm以下であった。
As described above, a polarization-maintaining optical fiber with a length of 10 km was manufactured and evaluated, and the transmission loss was found to be 1.
0.22dB/km 1 mode birefringence at 55mm is e
x to-' and eccentricity were less than 0.1 μm.

なお、本実施例においては、コア部、クラッド部及び応
力付与層の組成を、それぞれS+02−GeO2。
In this example, the compositions of the core part, cladding part, and stress applying layer are S+02-GeO2.

S10□、S10□−B203−P2O3としたが、こ
れに限られるものではな(、コア母材とクラッド母材の
組成を8102−GeO2−’P2O5とSiO゜、S
iO2と5IO2−F、5IO2GeO3とSiO2−
F、  及びSiO2−GeO2とSiO2−P20e
+−Fのいずれかとなし、応力付与層の組成を5IO2
−B203 、S IO□−B203−GeO2 、S
 102−B203−P 205 、S 102−B2
03A I 203 、S 102−F−A I 20
31S 102−F−P 20a +S 10.、−F
−GeO21SiO2−−TIO□及びTIO□−Fの
いずれかとしてもよい。
S10□, S10□-B203-P2O3, but it is not limited to this (, the composition of the core base material and clad base material is 8102-GeO2-'P2O5, SiO゜, S
iO2 and 5IO2-F, 5IO2GeO3 and SiO2-
F, and SiO2-GeO2 and SiO2-P20e
+-F, and the composition of the stress applying layer is 5IO2
-B203,S IO□-B203-GeO2,S
102-B203-P 205 , S 102-B2
03A I 203, S 102-F-A I 20
31S 102-F-P 20a +S 10. , -F
-GeO21SiO2--TIO□ or TIO□-F may be used.

又応力付与層の形成方法は、ガラス微粒子層の形成と同
時にSiO2−以外の添加剤を加える方法だけでなく、
ガラス微粒子層の焼結の際に添加剤を加える方法、ある
いは両者の併用も可能である。
In addition, the method for forming the stress imparting layer is not limited to adding additives other than SiO2- at the same time as forming the glass fine particle layer.
It is also possible to add additives during sintering of the glass fine particle layer, or to use both in combination.

(発明の効果) 以上説明したように、本発明の偏波面保存光ファイバの
製造方法によれば、次に列記するような効果を奏するも
のである。
(Effects of the Invention) As explained above, according to the method for manufacturing a polarization-maintaining optical fiber of the present invention, the following effects are achieved.

■コアロッドの楕円形状の均一化が容易になされ、特性
が向上する。
■The elliptical shape of the core rod can be easily made uniform, improving its characteristics.

■コアロッドを太くしてもクラックが発生することがな
く、長尺化が可能となる。
■Even if the core rod is made thicker, no cracks will occur, making it possible to make it longer.

■コアロッドを太くすることにより、コアロッドと応力
付与層との境界面におけるゆらぎの影響が緩和され、低
損失化が達成できる。
■By making the core rod thicker, the influence of fluctuations at the interface between the core rod and the stress-applying layer is alleviated, and lower loss can be achieved.

■コアロッドを楕円加工した後に応力付与層の外付けを
行なうので、光ファイバの偏心を小さくすることができ
る。
■Since the stress applying layer is attached externally after the core rod is processed into an ellipse, the eccentricity of the optical fiber can be reduced.

【図面の簡単な説明】[Brief explanation of drawings]

第1図(イ)〜(ネ)は本発明の偏波面保存光ファイバ
の製造方法の実施例に係る工程図である。 1・・・コア、2・・・クラッド、3・・・コアロッド
、4・・・ガラス微粒子層、5・・・応力付与層、6・
・・ジャケラ ト層。 悌 I 図 (イ) (ロ) (ノリ (ニ) (ホ)
FIGS. 1(A) to 1(N) are process diagrams relating to an embodiment of the method for manufacturing a polarization-maintaining optical fiber of the present invention. DESCRIPTION OF SYMBOLS 1... Core, 2... Clad, 3... Core rod, 4... Glass fine particle layer, 5... Stress imparting layer, 6...
...Jakerat layer.悌I fig (a) (b) (nori (d) (e)

Claims (4)

【特許請求の範囲】[Claims] (1)屈折率の高いコア部と、該コア部の屈折率よりも
屈折率の低いクラッド部から成るコアロッドを、断面略
楕円形状に研削加工した後、その外周部に応力付与層及
びジャケット層を順次形成し、ついで紡糸することを特
徴とする偏波面保存光ファイバの製造方法。
(1) A core rod consisting of a core portion with a high refractive index and a cladding portion with a refractive index lower than that of the core portion is ground into a substantially elliptical cross-section, and then a stress applying layer and a jacket layer are placed on the outer periphery of the core rod. 1. A method for producing a polarization-maintaining optical fiber, which comprises sequentially forming a polarization-maintaining optical fiber and then spinning the fiber.
(2)断面略楕円形状に研削加工したコアロッドの外周
部にガラス微粒子層を形成、焼結することにより応力付
与層となし、ついでコアロッド上に応力付与層を形成し
たガラス母材をジャケット層形成用ガラス管に挿入し一
体化後又は一体化と同時に紡糸することを特徴とする請
求項(1)記載の偏波面保存光ファイバの製造方法。
(2) A glass particle layer is formed on the outer periphery of a core rod that has been ground into a roughly elliptical cross-sectional shape and sintered to form a stress-applying layer, and then a jacket layer is formed using the glass base material with the stress-applying layer formed on the core rod. 2. The method for producing a polarization-maintaining optical fiber according to claim 1, wherein the fiber is inserted into a glass tube and spun after or simultaneously with the integration.
(3)断面略楕円形状に研削加工したコアロッドの外周
部にガラス微粒子層を形成、焼結して応力付与層及びジ
ャケット層を形成した後、紡糸することを特徴とする請
求項(1)記載の偏波面保存光ファイバの製造方法。
(3) A method according to claim (1), characterized in that a glass fine particle layer is formed on the outer periphery of a core rod that has been ground into a substantially elliptical cross-sectional shape, and after being sintered to form a stress applying layer and a jacket layer, spinning is performed. A method for manufacturing polarization-maintaining optical fiber.
(4)コア部及びクラッド部の組成をSiO_2−Ge
O_2とSiO_2、SiO_2−GeO_2−P_2
O_5とSiO_2、SiO_2とSiO_2−F、S
iO_2−GeO_2とSiO_2−F、及びSiO_
2−GeO_2とSiO_2−P_2O_5−Fのいず
れかとなし、応力付与層の組成をSiO_2−B_2O
_3、SiO_2−B_2O_3−GeO_2、SiO
_2−B_2O_3−P_2O_5、SiO_2−B_
2O_3−Al_2O_3、SiO_2−F−Al_2
O_3、SiO_2−F−P_2O_5、SiO_2−
F−GeO_2、SiO_2−TiO_2及びSiO_
2−TiO_2−Fのいずれかとなし、ジャケット層の
組成をクラッド部と同一とすることを特徴とする請求項
(1)〜(3)記載の偏波面保存光ファイバの製造方法
。
(4) The composition of the core part and cladding part is SiO_2-Ge.
O_2 and SiO_2, SiO_2-GeO_2-P_2
O_5 and SiO_2, SiO_2 and SiO_2-F, S
iO_2-GeO_2 and SiO_2-F, and SiO_
2-GeO_2 or SiO_2-P_2O_5-F, and the composition of the stress applying layer is SiO_2-B_2O.
_3, SiO_2-B_2O_3-GeO_2, SiO
_2-B_2O_3-P_2O_5, SiO_2-B_
2O_3-Al_2O_3, SiO_2-F-Al_2
O_3, SiO_2-F-P_2O_5, SiO_2-
F-GeO_2, SiO_2-TiO_2 and SiO_
2-TiO_2-F, and the composition of the jacket layer is the same as that of the cladding portion.
JP1327039A 1989-12-15 1989-12-15 Production of polarization maintaining optical fiber Ceased JPH03187942A (en)