JPH03189600A - Solidification of radioactive refuse - Google Patents
Solidification of radioactive refuseInfo
- Publication number
- JPH03189600A JPH03189600A JP32848389A JP32848389A JPH03189600A JP H03189600 A JPH03189600 A JP H03189600A JP 32848389 A JP32848389 A JP 32848389A JP 32848389 A JP32848389 A JP 32848389A JP H03189600 A JPH03189600 A JP H03189600A
- Authority
- JP
- Japan
- Prior art keywords
- specific gravity
- caking
- solidifying
- waste
- refuse
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Abstract
Description
【発明の詳細な説明】
〔産業上の利用分野〕
本発明は原子力発電所から発生する放射性廃棄物の固化
処理方法に係り、特に、水硬性の無機固化材を用いて固
化するのに好適な固化方法に関する。[Detailed Description of the Invention] [Field of Industrial Application] The present invention relates to a method for solidifying radioactive waste generated from nuclear power plants, and in particular, a method suitable for solidifying radioactive waste using a hydraulic inorganic solidifying material. Concerning solidification method.
従来、原子力発電所から発生する放射性廃棄物を固化容
器内に安定的に固化する固化材として、セメントをはじ
めとする無機の水硬性固化材が知られている。セント系
の固化材は、まず、低コストであること、無機材である
ため安定であること、操作が容易であること等数多くの
長所をもっている反面、固化体比重が2.0 を超え、
固化体重量は一体当たり約5百−と重く、固化体のハン
ドリングが容易ではない。BACKGROUND ART Conventionally, inorganic hydraulic solidifying materials such as cement have been known as solidifying materials that stably solidify radioactive waste generated from nuclear power plants in solidifying containers. First, cent-based solidifying materials have many advantages such as being low cost, being stable as an inorganic material, and being easy to operate.
The solidified mass is heavy, about 500 kg, and the solidified mass is not easy to handle.
一方、特開昭63−223598号公報に記載されてい
るように、固化材としてプラスチックを用いる方法があ
る。プラスチック系の固化材は、比重が1.5 前後で
あり、セメント系固化材に比較して固化体のハンドリン
グの面からは有利であるが、コストが高い、操作が複雑
等の不利な点もある。On the other hand, as described in Japanese Patent Application Laid-Open No. 63-223598, there is a method of using plastic as a solidifying material. Plastic-based solidifying materials have a specific gravity of around 1.5 and are advantageous in terms of handling of the solidified material compared to cement-based solidifying materials, but they also have disadvantages such as high cost and complicated operation. be.
北記従来技術のうち、セメント系の固化材は固化材の比
重について考慮されておらず、固化体をハンドリングし
にくいこと、あるいは、廃棄物が浮上する可能性がある
ため、その防止のための対立(金あみの設置)が必要で
あること等の問題があった。一方、プラスチック系の固
化材では、高コスト、操作の複雑さ、可燃性等の問題が
ある。Among the conventional technologies mentioned above, cement-based solidifying materials do not take into account the specific gravity of the solidifying material, making it difficult to handle the solidified material or causing waste to float to the surface. There were problems such as the necessity of confrontation (setting up gold nets). On the other hand, plastic solidifying materials have problems such as high cost, complexity of operation, and flammability.
本発明の目的は、セメント系の無機の固化材について、
その比重を固化する廃棄物の比重に合わせることにより
、廃棄物浮上に対する対策を不要とすることにある。The purpose of the present invention is to provide a cement-based inorganic solidifying material.
By adjusting the specific gravity to the specific gravity of the waste to be solidified, it is possible to eliminate the need for measures against the floating of waste.
本発明の他の目的は、廃棄物の比重は概してセント系固
化材の比重より小さいことから、固化付比重を廃棄物の
比重に合わせることにより、固化体を軽量にしハンドリ
ングを容易にすることにある。Another object of the present invention is to make the solidified material lighter and easier to handle by adjusting the solidification specific gravity to the specific gravity of the waste, since the specific gravity of waste is generally smaller than the specific gravity of cent-based solidifying materials. be.
C課題を解決するための手段〕
本発明では、上記目的を達成するために、固化材より比
重の小さい無機材、好ましくは、その微粉末を固化材に
添加したものである。あるいは、上記目的を達成するた
めに、発泡性の薬剤(空気連行剤)を添加するか、起泡
した泡を固化材ペーストと混合したものである。Means for Solving Problem C] In the present invention, in order to achieve the above object, an inorganic material having a specific gravity lower than that of the solidifying material, preferably a fine powder thereof, is added to the solidifying material. Alternatively, in order to achieve the above object, a foaming agent (air entraining agent) is added or foamed foam is mixed with a solidifying material paste.
上記無機材には、比重1.0 前後の人工超軽量骨材が
適する。発泡性の薬剤には、リグニンスルホン酸塩、オ
キシ有機酸塩、アルキルアリルスルホン酸塩等を主成分
とする空気連行剤(AE剤)、やポリオキシエチレンア
ルキルエーテル、樹脂せっけん系、加水分解たん白系等
の起泡剤が適する。An artificial ultra-light aggregate with a specific gravity of around 1.0 is suitable for the above-mentioned inorganic material. Foaming agents include air entraining agents (AE agents) whose main ingredients are lignin sulfonates, oxyorganic acid salts, alkylaryl sulfonates, etc., polyoxyethylene alkyl ethers, resin soaps, and hydrolyzed proteins. White foaming agents are suitable.
その他の起泡方法は、起泡液を圧さく空気により噴出さ
せる発泡機を用いる方法があり、生成された泡を固化材
ペーストと混合することにより、発泡性薬剤の添加と同
様の効果が得られる。Another foaming method is to use a foaming machine that compresses the foaming liquid and blows it out with air. By mixing the generated foam with the solidifying material paste, the same effect as adding a foaming agent can be obtained. It will be done.
固化材より低比重の無機材は固化付比重を小さくする働
きがあり、その添加量を調整することにより固化対象廃
棄物の比重に固化付比重を合わせることができる。Inorganic materials having a lower specific gravity than the solidification material have the function of reducing the specific gravity for solidification, and by adjusting the amount added, the specific gravity for solidification can be matched to the specific gravity of the waste to be solidified.
発泡剤は、固化体の中に独立気泡を多数、人工的に生成
させ固化付比重を下げる働きがあり、その添加量や混線
方法により連行空気量を制御して固化付比重を廃棄物の
比重に合わせることができる。発泡機を用いる方法も同
様であり、固化材ペースト中の気泡量を制御することに
より、固化付比重を調整することができる。A blowing agent has the function of artificially creating a large number of closed cells in the solidified material to lower the specific gravity of the solidified material, and by controlling the amount of air entrained by the amount of addition and the mixing method, the specific gravity of the solidified material can be adjusted to the specific gravity of the waste. It can be adjusted to The method using a foaming machine is also similar, and the solidification specific gravity can be adjusted by controlling the amount of bubbles in the solidification material paste.
〈実施例1〉
本発明の一実施例を第1図により説明する。本実施例は
放射性廃棄物の造粒体を充てんした容器にセメント系の
固化材を注入して固化するのに好適な方法である。通常
は、混練槽1へ混練水タンク2より混練水が、固化材タ
ンク3よりフィーダ5を介して固化材が供給され固化材
ペーストを作成する。ここで本発明では固化容器6へあ
らかじめ充てんされた廃棄物ペレット7の比重を計測し
ておき、固化材ペーストの比重をペレットの比重と同等
もしくはその近傍の値に調整するために必要な量の軽量
骨材を骨材貯槽4よりフィーダ5を介して混練槽1へ供
給する。十分混練された固化材ペーストはバルブを介し
て、固化容器6へ注入され、所定期間養生して固化体8
となって搬出される。<Example 1> An example of the present invention will be described with reference to FIG. This embodiment is a suitable method for injecting a cement-based solidifying material into a container filled with radioactive waste granules and solidifying them. Normally, kneading water is supplied from a kneading water tank 2 to a kneading tank 1, and solidifying material is supplied from a solidifying material tank 3 via a feeder 5 to create a solidifying material paste. Here, in the present invention, the specific gravity of the waste pellets 7 filled into the solidification container 6 is measured in advance, and the amount necessary to adjust the specific gravity of the solidification material paste to a value equal to or close to the specific gravity of the pellets is measured. Light aggregate is supplied from an aggregate storage tank 4 to a kneading tank 1 via a feeder 5. The sufficiently kneaded solidifying material paste is injected into the solidifying container 6 through a valve, and is cured for a predetermined period to form a solidified material 8.
It is then carried out.
次に本実施例を具体的に説明する。使用した固化材は普
通ポル1へランドセメント(比重3.15)、廃棄物ペ
レットの比重は1.53 であった。そこで次の組成の
ペーストを作成し、廃棄物ペレットを充てんした容器に
注入した。なお、使用した骨材は人工軽量骨材であり、
その比重は1.20であった。Next, this example will be explained in detail. The solidifying material used was ordinary Pol 1 heland cement (specific gravity 3.15), and the specific gravity of the waste pellets was 1.53. Therefore, a paste with the following composition was prepared and poured into a container filled with waste pellets. The aggregate used was an artificial lightweight aggregate.
Its specific gravity was 1.20.
ポルトランドセメント 60kg
混練水 40kg
骨材 40kg
上記組成のペーストは、比重が1.52であり、廃棄物
ペレットの比重とほぼ同等であった。そのため、ペース
ト注入時のペレットの浮上はなく。Portland cement 60 kg Mixing water 40 kg Aggregate 40 kg The paste with the above composition had a specific gravity of 1.52, which was almost the same as the specific gravity of waste pellets. Therefore, there is no floating of pellets during paste injection.
ペレットが均一に分布した良好な固化体を作成すること
かできた。比較のために作成した骨材無添加のポルトラ
ンドセメントによる同体積の固化体と比較して、固化体
重量は、約32%軽量化された。It was possible to create a good solidified material in which the pellets were uniformly distributed. The solidified weight was approximately 32% lighter compared to a solidified body of the same volume made of Portland cement without aggregate added, which was prepared for comparison.
本実施例では、廃棄物の比重が異なれば骨材の比重、あ
るいは、その添加量を調整することにより対応でき、固
化材より低比重の廃棄物の固化処理に広く適用可能であ
る。In this embodiment, if the specific gravity of the waste differs, it can be handled by adjusting the specific gravity of the aggregate or the amount added thereof, and it is widely applicable to the solidification treatment of waste having a lower specific gravity than the solidifying material.
〈実施例2〉 本発明の次の実施例を第2図を用いて説明する。<Example 2> The next embodiment of the present invention will be described with reference to FIG.
本実施例では、固化材ペースト中に気泡を生成させて固
化材ペーストの比重を調整する。第2図に示すように、
骨材貯槽の代わりに発泡機9を設置する。発泡機は起泡
剤を圧さく空気によりノズルから噴出させ泡を発生させ
る。発生した泡は混線機1内で予め混練されている固化
材ペーストに導入され、混合される。この際の空気連行
量は、ペーストの体積増分から求めることができる。こ
の際、固化する廃棄物の比重と固化材ペーストの比重を
合わせるために空気連行量を制御する。In this embodiment, air bubbles are generated in the solidifying material paste to adjust the specific gravity of the solidifying material paste. As shown in Figure 2,
A foaming machine 9 is installed in place of the aggregate storage tank. A foaming machine generates foam by squirting a foaming agent out of a nozzle using compressed air. The generated bubbles are introduced into the solidifying material paste that has been kneaded in advance in the mixer 1 and mixed therein. The amount of air entrained at this time can be determined from the volume increase of the paste. At this time, the amount of air entrainment is controlled in order to match the specific gravity of the waste to be solidified and the specific gravity of the solidifying material paste.
次に、本実施例を具体的に説明する。固化材は普通ポル
トランドセメントである。固化した廃棄物ペレットの比
重は1.35であった。予め、固化材ペーストを次の組
成で混練した。Next, this example will be explained in detail. The solidifying material is usually Portland cement. The specific gravity of the solidified waste pellets was 1.35. A solidifying material paste was kneaded in advance with the following composition.
ポルトランドセメント 100kg
混練水 50kg
その後、発泡機により空気連行量を25%となるまで気
泡を固化材ペーストへ導入させた。この操作により、固
化材ペーストの比重を1.33 に調整することができ
た。そのため、廃棄物ペレットの浮上は見られず、均一
に固化体内に分布していた。固化体重量は気泡のない場
合に比べて約30%軽量化された。Portland cement 100 kg Kneading water 50 kg Thereafter, air bubbles were introduced into the solidifying material paste using a foaming machine until the amount of air entrainment reached 25%. Through this operation, the specific gravity of the solidifying material paste could be adjusted to 1.33. Therefore, no floating of the waste pellets was observed, and they were uniformly distributed within the solidified body. The solidified weight was reduced by about 30% compared to the case without bubbles.
本発明によれば、固化材と廃棄物の比重差を小さくでき
るので、廃棄物の浮上を防止できる効果がある。According to the present invention, since the difference in specific gravity between the solidifying material and the waste can be reduced, there is an effect that floating of the waste can be prevented.
また、固化材が軽量化されるため、固化材のハンドリン
グのための負荷を軽減できる効果がある。Furthermore, since the weight of the solidified material is reduced, the load for handling the solidified material can be reduced.
第1図は本発明の一実施例の処理フローの説明図、第2
図は本発明の他の実施例の処理フローの説明図である。
1・・混練機、4・・・骨材貯槽、5・・フィーダー、
6第1図FIG. 1 is an explanatory diagram of the processing flow of an embodiment of the present invention, and FIG.
The figure is an explanatory diagram of the processing flow of another embodiment of the present invention. 1. Kneading machine, 4. Aggregate storage tank, 5. Feeder,
6Figure 1
Claims (1)
内に固化する際に、前記固化材の比重を前記廃棄物の比
重と同等もしくはその近傍とすることを特徴とする放射
性廃棄物の固化方法。 2、放射性廃棄物を水硬性の固化材を用いて固化容器内
に固化する際に、前記固化材より比重の小さい無機材を
前記固化材に添加することにより前記固化材の比重を廃
棄物の比重と同等もしくはその近傍とすることを特徴と
する放射性廃棄物の固化方法。 3、放射性の廃棄物を水硬性の固化材を用いて固化容器
内に固化する際に、発泡性の薬剤を添加するか、または
、起泡された泡を前記固化材のペースト中に混合するこ
とにより前記固化材の比重の前記廃棄物の比重と同等も
しくはその近傍とすることを特徴とする放射性廃棄物の
固化方法。[Claims] 1. When radioactive waste is solidified in a solidification container using a hydraulic solidification material, the specific gravity of the solidification material is set to be equal to or close to the specific gravity of the waste. A distinctive method of solidifying radioactive waste. 2. When solidifying radioactive waste in a solidifying container using a hydraulic solidifying material, by adding an inorganic material with a smaller specific gravity than the solidifying material to the solidifying material, the specific gravity of the solidifying material is lower than that of the waste. A method of solidifying radioactive waste characterized by making the specific gravity equal to or close to it. 3. When solidifying radioactive waste in a solidification container using a hydraulic solidification material, a foaming agent is added or the foamed foam is mixed into the paste of the solidification material. A method for solidifying radioactive waste, characterized in that the specific gravity of the solidifying material is equal to or close to the specific gravity of the waste.