JPH03220399A - Production of sheet for stamp and sheet for stamp - Google Patents

Production of sheet for stamp and sheet for stamp

Info

Publication number
JPH03220399A
JPH03220399A JP32443890A JP32443890A JPH03220399A JP H03220399 A JPH03220399 A JP H03220399A JP 32443890 A JP32443890 A JP 32443890A JP 32443890 A JP32443890 A JP 32443890A JP H03220399 A JPH03220399 A JP H03220399A
Authority
JP
Japan
Prior art keywords
inorganic fluorescent
fluorescent pigment
stamp
stamp sheet
pigment
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP32443890A
Other languages
Japanese (ja)
Other versions
JP2676712B2 (en
Inventor
Shigeji Matsuzawa
茂治 松澤
Eiji Yuasa
栄治 湯浅
Junichiro Tanaka
淳一郎 田中
Teruo Nakamura
中村 照雄
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kanzaki Paper Manufacturing Co Ltd
Original Assignee
Kanzaki Paper Manufacturing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kanzaki Paper Manufacturing Co Ltd filed Critical Kanzaki Paper Manufacturing Co Ltd
Priority to JP2324438A priority Critical patent/JP2676712B2/en
Publication of JPH03220399A publication Critical patent/JPH03220399A/en
Application granted granted Critical
Publication of JP2676712B2 publication Critical patent/JP2676712B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

PURPOSE:To obtain the subject sheet having excellent appearance and printability with improved working efficiency by applying a coating solution containing pigment, inorganic fluorescent pigment after a specific treatment and adhesive as principal components on a supporting body and drying. CONSTITUTION:Inorganic fluorescent pigment (preferably fluorescent pigment to be excited by irradiation of light having 254 or 356nm wavelength) is subjected to wet crushing treatment in a sand mill, etc., so as to have specific surface area satisfying a condition expressed by the formula (Sw1 is specific surface area after the wet crushing treatment; Sw2 is specific surface area before the wet crushing treatment) to produce dispersion of the fluorescent pigment. Then, said dispersion is mixed with general pigment such as kaolin in an amount of 0.5-4.0wt.% of total pigment component, adhesive such as casein and various auxiliaries such as lubricant or water-retentive agent, thus applied to a supporting body in an amount of 5-30g/m per one face in dried weight so as to give <=1000mug worn degree of a stamp sheet to afford the aimed sheet.

Description

【発明の詳細な説明】 (産業上の利用分野) 本発明は、切手用シートの製造方法及び切手用シートに
関し、特に無機蛍光顔料を含有する切手用シートの製造
方法及び切手用シートに関するものである。
Detailed Description of the Invention (Field of Industrial Application) The present invention relates to a method for producing a stamp sheet and a stamp sheet, and particularly relates to a method for producing a stamp sheet containing an inorganic fluorescent pigment and a stamp sheet. be.

(従来の技術) 従来から、切手は世界各国で発行され、デザイン、寸法
や素材等その国独特の特色ある、美しい切手が創り出さ
れている。
(Prior art) Stamps have traditionally been issued in countries around the world, creating beautiful stamps with unique characteristics unique to each country, such as design, dimensions, and materials.

近年、郵便物の増加と共に、その取扱い量も極めて多く
なっている。そのために、能率的な処理、業務を遂行で
きるように郵便物処理の機械処理が進んでいる。
In recent years, as the number of mail items has increased, the amount of mail handled has also increased significantly. For this reason, mechanical processing of mail is progressing to enable efficient processing and business execution.

その中の1つに、郵便物の切手によって判別、処理を行
う検知方式がいろいろ採用されている。
One of these methods is the use of various detection methods that identify and process mail based on stamps.

その検知手段として、例えば切手自体に別色する方法、
蛍光顔料−特に無機蛍光顔料を付与して、その蛍光発色
を利用して、検出器にて切手の貼付の有無や自動正置、
及び押印等の業務改善が図られている。
As a means of detecting this, for example, a method of painting the stamp itself in a different color,
Fluorescent pigments, especially inorganic fluorescent pigments, are applied and the fluorescence is used to detect whether or not stamps are affixed, automatic alignment, etc. using a detector.
Improvements are being made to improve operations such as stamping and stamping.

そして、蛍光材料を用いた切手、所謂発光切手と呼ばれ
る切手を製造する場合、その製造方法として、例えば切
手を印刷するための印刷用インキ内に無機蛍光顔料を練
り込み、グラビア印刷機で印刷する方法がある。ところ
が、このインキを紙面上に印刷する場合にグラビアロー
ルに付着したインキのうち過剰分のインキを取り除(の
に、通常は掻き落し刃が使用されるが、インキ中の無機
蛍光顔料の分散性が不十分なために掻き落とす際に微細
スクラッチ(微細なひっかき状の筋)が多発し、これが
そのまま紙面に転移され、外観及び印刷適性不良といっ
た問題が生じている。
When manufacturing stamps using fluorescent materials, so-called luminescent stamps, the manufacturing method involves, for example, kneading an inorganic fluorescent pigment into the printing ink used to print the stamps and printing with a gravure printing machine. There is a way. However, when printing this ink on paper, a scraping blade is usually used to remove the excess ink that adheres to the gravure roll, but it is difficult to disperse the inorganic fluorescent pigment in the ink. Due to the insufficient properties, many fine scratches (fine scratch-like streaks) occur during scraping, and these are transferred directly to the paper surface, resulting in problems such as poor appearance and printability.

なお、上記の難点を回避する方法として、無機蛍光顔料
をインキ中に含有させる代わりに、切手の構成成分であ
る支持体の塗被層中に含有させる方法もある。この場合
、切手に仕上げる前段階として無機蛍光顔料を含有する
顔料塗被液を各種のコーターで支持体に塗布して切手用
塗被紙を作製するが、インキの場合と同様に、塗被液中
の無機蛍光顔料の粗粒子が悪影響を及ぼし、塗被適性を
低下させ、さらに得られた塗被紙のグラビア印刷適性(
主にミスト、ト)不良等の難点がある。
In addition, as a method to avoid the above-mentioned drawbacks, there is also a method of including the inorganic fluorescent pigment in the coating layer of the support, which is a constituent component of the stamp, instead of including the inorganic fluorescent pigment in the ink. In this case, as a step before finishing the stamp, a pigment coating liquid containing an inorganic fluorescent pigment is applied to the support using various coaters to prepare coated paper for stamps. The coarse particles of the inorganic fluorescent pigment inside have an adverse effect, lowering the coating suitability, and further affecting the gravure printing suitability of the resulting coated paper (
Mainly, there are drawbacks such as mist and defects.

また、無機蛍光顔料は他の塗被紙用顔料、例えば炭酸カ
ルシウム等と比較して硬いために、切手製品の断裁やタ
ック加工された切手製品のグイカント時にカッティング
刃の著しい磨耗を招き、作業能率を低下させる原因とな
っている。
In addition, because inorganic fluorescent pigments are harder than other coated paper pigments, such as calcium carbonate, they cause significant wear on the cutting blade when cutting stamp products or when tucking stamp products that have been tacked, resulting in reduced work efficiency. This causes a decrease in

(発明が解決しようとする課題) 本発明は、無機蛍光顔料を塗被液に含有させることに起
因する塗被液の塗被適性の低下、特にプレートコータ等
で発生する微細スクラッチトラブルやストリーク等の条
跡トラブルを効果的に解消し、しかも、切手用として塗
被、製品仕上げされた後に、印刷、小断ち断裁やグイカ
ッティング等の、所謂用途目的に合わせて種々の加工が
施されるが、この場合、カッティング刃の摩耗性の改善
及び印刷適性(グラビア印I1)時のミスドツト)の改
良された高品質の切手用シートを極めて効率良く製造す
る方法、並びにかかる方法で製造される高品質の切手用
シートを提供するものである。
(Problems to be Solved by the Invention) The present invention aims to reduce the coating suitability of the coating liquid due to the inclusion of an inorganic fluorescent pigment in the coating liquid, and to solve problems such as fine scratch troubles and streaks that occur in plate coaters, etc. Moreover, after being coated and finished for stamps, various processes are performed to suit the purpose of use, such as printing, small cutting, and cutting. , in this case, a method for extremely efficiently producing a high-quality stamp sheet with improved abrasion properties of the cutting blade and printability (misdots during gravure printing I1), and a high-quality stamp sheet produced by such a method. The company provides sheets for stamps.

(課題を解決するための手段) 本発明は、支持体上に、顔料、無機蛍光顔料及び接着剤
を主成分とする塗被液を塗被、乾燥して得る切手用シー
トの製造方法において、予め、下記条件を満たす比表面
積となるように無機蛍光顔料を湿式粉砕処理し、処理後
の無機蛍光顔料分散液を塗被液に配合することを特徴と
する切手用シトの製造方法、並びにかかる方法で製造さ
れる切手用シートである。
(Means for Solving the Problems) The present invention provides a method for producing a stamp sheet obtained by coating a support with a coating liquid containing a pigment, an inorganic fluorescent pigment, and an adhesive as main components and drying the coating liquid. A method for producing a sheet for stamps, which comprises wet-pulverizing an inorganic fluorescent pigment in advance so that it has a specific surface area that satisfies the following conditions, and blending the treated inorganic fluorescent pigment dispersion into a coating liquid; This is a stamp sheet manufactured by the method.

2.0≧Sw+/Swz≧1.05 上記式中、 $−1=湿式粉砕処理後の比表面積 S−2:湿式粉砕処理前の比表面積 (単位: c m” /g) (作用) 発光切手に使用される無機蛍光顔料は、−iに単一粒子
径としては2μm前後のものであるが、その水分散液は
二次凝集を起こし易く、水中では会合して10μmから
、大きいものになると50μmを越すような粗粒子とな
っていることが本発明者等の検討によって明らかとなっ
た。
2.0≧Sw+/Swz≧1.05 In the above formula, $-1=specific surface area after wet pulverization S-2: specific surface area before wet pulverization (unit: cm”/g) (effect) Luminescence The inorganic fluorescent pigment used in stamps has a single particle size of around 2 μm, but its aqueous dispersion tends to cause secondary aggregation, and in water it aggregates and grows into larger particles from 10 μm. The inventors' studies have revealed that this results in coarse particles exceeding 50 μm.

そのため、無機蛍光顔料の二次凝集による粗粒子を解離
するためにケーディミルやコーレスディゾルバー等の強
力な撹拌機を用いて分散を試みたが、二次凝集物の解離
は殆ど行われず、効果の少ないことが判った。このため
、アトライター、サンドミル、グイノーミル等と言われ
る、所謂ビーズと顔料を一緒に機械撹拌し、ビーズと顔
料或いは顔料同士の摩擦や衝突の繰り返しによって顔料
を微細化する湿式粉砕機に着目し、この装置で無機蛍光
顔料を特定の比表面積まで処理して得られる分散液を塗
被液中に配合すると、スクラッチやストリーク等の条跡
トラブルが完全シこ解消できることが判った。
Therefore, in order to dissociate the coarse particles caused by the secondary aggregation of inorganic fluorescent pigments, attempts were made to disperse them using powerful stirrers such as Kade Mill and Coles Dissolver, but the dissociation of the secondary agglomerates was hardly achieved and the effect was low. It turned out that. For this reason, we focused on wet grinders such as attritors, sand mills, and guino mills, which mechanically stir beads and pigments together and atomize the pigments through repeated friction and collision between the beads and pigments or between pigments. It has been found that when a dispersion obtained by processing an inorganic fluorescent pigment to a specific surface area using this device is blended into a coating liquid, problems with streaks such as scratches and streaks can be completely eliminated.

また、上記の如き湿式粉砕処理を施した無機蛍光顔料の
分散液を切手用シートの塗被層を形成する塗被液中に特
定量配合することにより、得られる切手用シートの摩耗
度を特定値以下Sこ調整すると、カッティング刃の磨耗
の進行が極端に遅くなり、カッティング作業適性が極め
て効果的に改良されることも明らかとなった。
In addition, by blending a specific amount of a dispersion of an inorganic fluorescent pigment that has been subjected to the wet pulverization process as described above into the coating liquid that forms the coating layer of the stamp sheet, the degree of wear of the resulting stamp sheet can be determined. It has also become clear that when the value S is adjusted below this value, the progress of wear of the cutting blade is extremely slowed down, and the suitability for cutting work is extremely effectively improved.

さらに、例えば重質炭酸カルシウムの場合、湿式粉砕処
理をすると、その理由は明らかではないが、グラビア印
刷におけるミスドツトが悪化する傾向にある。しかし、
本発明における無機蛍光顔料の場合にはミスドツトの発
生が著しく軽減されることが明らかとなった。
Furthermore, for example, in the case of heavy calcium carbonate, wet pulverization tends to worsen misdots in gravure printing, although the reason is not clear. but,
It has become clear that the occurrence of misdots is significantly reduced in the case of the inorganic fluorescent pigment of the present invention.

なお、湿式粉砕処理は各種顔料の微粉砕方法として知ら
れているが、本発明の方法では、上記の如くその処理条
件を特定し、且つそのような特定の条件下で処理された
無機蛍光顔料の分散液を、直接、切手用シートの塗被層
を形成する塗被液中に特定量配合することによって、塗
被液の塗被適性を改良するのみならず、得られる切手用
シートの品質適性をも顕著に改良せしめているものであ
る。
Note that wet pulverization is known as a method for pulverizing various pigments, but in the method of the present invention, the processing conditions are specified as described above, and inorganic fluorescent pigments treated under such specific conditions are used. By directly blending a specific amount of the dispersion into the coating liquid that forms the coating layer of the stamp sheet, not only the coating suitability of the coating liquid is improved, but also the quality of the resulting stamp sheet is improved. It also significantly improves aptitude.

そのため、本発明の方法では無機蛍光顔料の水分散液を
湿式粉砕処理するに際し、無機蛍光顔料の比表面積が下
記式を満足するように処理する必要がある。
Therefore, in the method of the present invention, when wet-pulverizing an aqueous dispersion of an inorganic fluorescent pigment, it is necessary to perform the treatment so that the specific surface area of the inorganic fluorescent pigment satisfies the following formula.

2.0≧Sw+/Sing≧1.05 上記式中、 Sw、 :湿式粉砕処理後の比表面積 Sw2:湿式粉砕処理前の比表面積 (単位: c m” /g) 因に、S賀+/SWzが1.05未満の場合には、無機
蛍光顔料の二次凝集による粗大粒子の解離が不完全とな
り、スクラッチの解消効果や摩耗性及び印刷通性(グラ
ビア印刷におけるミスドツト)の改善の効果が期待でき
ない。一方、2.0を越えると、蛍光発色強度が低下し
、切手用シート本来の品質に難点を生じるおそれがある
。
2.0≧Sw+/Sing≧1.05 In the above formula, Sw: Specific surface area after wet pulverization Sw2: Specific surface area before wet pulverization (unit: cm”/g) If SWz is less than 1.05, the dissociation of coarse particles due to secondary aggregation of the inorganic fluorescent pigment will be incomplete, and the effect of eliminating scratches and improving abrasion resistance and printing permeability (misdots in gravure printing) will be insufficient. On the other hand, if it exceeds 2.0, the fluorescent coloring intensity decreases, which may cause problems in the original quality of the stamp sheet.

而して、本発明の方法で使用される湿式粉砕装置として
;よ、前記の如く、例えばアトライターサンドミル、ダ
イノーミル等があるが、特にサンドミルやダイノーミル
(横型サンドミルの代表的な商品名)は、粗大粒子の選
択的な粉砕効果に優れているため好まじく用いられる。
As mentioned above, the wet grinding apparatus used in the method of the present invention includes, for example, the attriter sand mill and the Dyno mill, but in particular, the sand mill and the Dyno mill (a typical trade name for horizontal sand mills) are as follows: It is preferably used because it has an excellent selective crushing effect on coarse particles.

サンドミルやダイノーミルに使用される微小粒子(ビー
ズ)の平均粒径は、約3mm程度以下であり、その材質
としては天然、合成の鉱物、微小砂、硬質ガラス、硬質
プラスチック、金属等がある。これらの微小粒子は、容
器中に一定量投入され、外部から導入される被処理分散
液の粒子と一諸に機械的に撹拌されるが、処理分散液は
容器中を通過ないし還流して微粉砕処理される。
The average particle size of the microparticles (beads) used in sand mills and dyno mills is approximately 3 mm or less, and their materials include natural and synthetic minerals, fine sand, hard glass, hard plastic, and metal. A certain amount of these microparticles are put into a container and are mechanically stirred together with the particles of the dispersion to be treated introduced from the outside, but the treated dispersion passes or refluxes through the container and becomes fine. Processed by crushing.

なお、粉砕方法には乾式粉砕法もあるが、本発明で使用
される無機蛍光顔料の粉砕には適しておらず、このよう
な粉砕方法では、本発明の所望の効果を得ることはでき
ない。
Although there is a dry pulverization method as a pulverization method, it is not suitable for pulverizing the inorganic fluorescent pigment used in the present invention, and such a pulverization method cannot achieve the desired effect of the present invention.

また、本発明の方法においては、上記の如く、無機蛍光
顔料の粉砕程度をその比表面積によって測定するが、こ
の場合の比表面積は恒圧通気式粉体比表面積測定法によ
って測定される。
Further, in the method of the present invention, as described above, the degree of pulverization of the inorganic fluorescent pigment is measured by its specific surface area, and the specific surface area in this case is measured by a constant pressure aeration powder specific surface area measurement method.

本発明において使用される無機蛍光顔料としては、例え
ばZnz S ioa:Mn (緑色発光)、CaS 
io=: pb :Mn (赤色発光)、ZnS:Cu
(緑色発光)等が挙げられるが、特に切手用シートとし
ての特性上、254或は356nmの波長を照射した時
に励起される蛍光顔料が好ましく使用される。
Examples of inorganic fluorescent pigments used in the present invention include Znz Sioa:Mn (green luminescence), CaS
io=: pb:Mn (red emission), ZnS:Cu
(emitting green light), etc., but fluorescent pigments that are excited when irradiated with wavelengths of 254 or 356 nm are preferably used, particularly in view of their properties as stamp sheets.

無機蛍光顔料の水分散液は固形分濃度が30〜60重量
%の分散液として湿式粉砕処理に掛けられる。
An aqueous dispersion of an inorganic fluorescent pigment is subjected to a wet grinding treatment as a dispersion having a solid content concentration of 30 to 60% by weight.

分散液の調製にあたっては、一般に塗被紙用顔料の分散
に用いられるポリアクリル酸ナトリウム、リグニンスル
ホン酸ナトリウム、リン酸塩、オレフィン無水マレイン
酸共重合体、クエン酸ナトリウム、コハク酸ナトリウム
等の分散剤の一種以上を必要シこ応して使用することが
できる。さらに、保護コロイドとして、澱粉、PVA等
を併用することも可能である。
In preparing the dispersion, sodium polyacrylate, sodium lignin sulfonate, phosphate, olefin maleic anhydride copolymer, sodium citrate, sodium succinate, etc., which are generally used for dispersing pigments for coated paper, are dispersed. One or more of these agents can be used as required. Furthermore, it is also possible to use starch, PVA, etc. in combination as a protective colloid.

本発明の方法では、かくして特定の湿式粉砕処理を施さ
れた無機蛍光顔料の分散液を、切手用シトの塗被層を形
成する塗被液中に配合せしめるものであるが、その配合
量は得られる切手用シートの摩耗度との兼ね合いで重要
であり、塗被液を構成する全顔料成分の0.5〜4.0
重量%、好ましくは1.0〜3.0重量%の範囲で調節
する必要がある。
In the method of the present invention, a dispersion of an inorganic fluorescent pigment that has been subjected to a specific wet pulverization treatment is blended into a coating liquid that forms the coating layer of a stamp sheet. This is important in terms of the degree of abrasion of the obtained stamp sheet, and it is important that the amount of pigments in the coating liquid is 0.5 to 4.0.
It is necessary to adjust the amount by weight, preferably within the range of 1.0 to 3.0 weight%.

因に、0.5重量%未満では発光性が低下し、発光切手
シートとして要求される検知適性に欠け、4.0重量%
を越えると湿式粉砕処理を施しても、得られる塗被液の
塗被適性が低下し、所望の摩耗度を得るのが難しくなる
おそれがある。
Incidentally, if it is less than 0.5% by weight, the luminescence property decreases and the detection suitability required for a luminescent stamp sheet is lacking, and if it is less than 0.5% by weight,
If it exceeds this amount, even if wet pulverization is performed, the coating suitability of the resulting coating liquid will be reduced, and it may become difficult to obtain a desired degree of abrasion.

なお、塗被液を構成する一般顔料としては、例えばクレ
ー、カオリン、水酸化アルミニウム、炭酸カルシウム、
二酸化チタン、硫酸バリウム、酸化亜鉛、サテンホワイ
ト、硫酸カルシウム、タルク、プラスチックピグメント
等の如き通常の塗被紙用顔料が挙げられるが、これらは
二種以上を適宜併用することも可能である。
Examples of general pigments constituting the coating liquid include clay, kaolin, aluminum hydroxide, calcium carbonate,
Typical pigments for coated paper include titanium dioxide, barium sulfate, zinc oxide, satin white, calcium sulfate, talc, plastic pigments, etc., but two or more of these may be used in combination as appropriate.

接着剤としては、例えばカゼイン、大豆蛋白、合成蛋白
等の蛋白質類;スチレン−ブタジェン共重合体、メチル
メタクリレート−ブタジェン共重合体等の共役ジエン系
重合体ラテックス、アクリル酸エステル及び/又はメタ
クリル酸エステルの重合体又は共重合体等のアクリル系
重合体ラテンクス、エチレン−酢酸ビニル共重合体等の
ビニル系重合体ラテックス、或いはこれらの各種重合体
をカルボキシル基等の官能基含有単量体で変性じたアル
カリ溶解性或いはアルカリ非溶解性の重合体ラテックス
;ポリビニルアルコール、オレフィン−無水マレイン酸
樹脂、メラミン樹脂等の合成樹脂系接着剤;陽性化澱粉
、酸化澱粉等の澱粉類;カルボキシメチルセルロース、
ヒドロキシエチルセルロース等のセルロース誘導体等の
如き通常の塗被紙用塗被液に用いられる接着剤の一種以
上が適宜選択して使用される。
Examples of adhesives include proteins such as casein, soybean protein, and synthetic proteins; conjugated diene polymer latex such as styrene-butadiene copolymer and methyl methacrylate-butadiene copolymer; acrylic esters and/or methacrylic esters. Acrylic polymer latices such as polymers or copolymers of alkali-soluble or alkali-insoluble polymer latex; synthetic resin adhesives such as polyvinyl alcohol, olefin-maleic anhydride resin, and melamine resin; starches such as positive starch and oxidized starch; carboxymethyl cellulose,
One or more adhesives, such as cellulose derivatives such as hydroxyethyl cellulose, which are commonly used in coating liquids for coated paper, are appropriately selected and used.

また、一般に塗被紙用組成物に用いろれる流動変性剤、
消泡剤、染料、滑剤、耐水化剤、保水剤等の各種助剤を
用いることも何等妨げるものではない。
In addition, flow modifiers generally used in coated paper compositions,
There is nothing that precludes the use of various auxiliary agents such as antifoaming agents, dyes, lubricants, waterproofing agents, and water retention agents.

本発明において、無機蛍光顔料の分散液を含む塗被液の
支持体への塗被方法は特に限定されないが、ブレード塗
工方法は、均一で平滑な塗被面の形成が容易であり、し
かも、本発明の方法では塗被液の塗被適性が効率良く改
良されているため、かかる塗工方法の適用は本発明の好
ましい実晦態様の一つである。
In the present invention, the method for applying the coating liquid containing the dispersion of the inorganic fluorescent pigment to the support is not particularly limited, but the blade coating method can easily form a uniform and smooth coated surface. Since the method of the present invention efficiently improves the coating suitability of the coating liquid, application of this coating method is one of the preferred embodiments of the present invention.

なお、塗被液の支持体への塗被量は、乾燥重量で片面当
たり5〜30 g / m、好ましくは8〜25g/m
程度の範囲で調節するのが望ましい。また、支持体につ
いては特に限定されないが、例えば紙を使用する場合に
は、酸性或いはアルカリ性条件下で抄紙された上質紙や
中質紙等が適宜選択して使用される。
The coating amount of the coating liquid on the support is 5 to 30 g/m per side, preferably 8 to 25 g/m in terms of dry weight.
It is desirable to adjust within a range of degrees. Further, the support is not particularly limited, but when paper is used, for example, wood-free paper or medium-quality paper made under acidic or alkaline conditions is appropriately selected and used.

ところで、得られる切手シートの摩耗度は以下の如き方
法で測定される。
Incidentally, the degree of wear of the obtained stamp sheet is measured by the following method.

即ち、10枚重ねたシートに一定条件下で真鍮針(組成
Cu/Zn =58/42)によって、異なる個所に1
0000回穴を開け、この操作を行う前後の真鍮針の重
量差を求めて、その値を摩耗度(μg)とした。
That is, 10 stacked sheets were pierced at different locations under certain conditions using a brass needle (composition Cu/Zn = 58/42).
A hole was punched 0,000 times, and the difference in weight of the brass needle before and after this operation was determined, and the value was taken as the degree of wear (μg).

本発明の方法では、特定の湿式粉砕処理を施された無機
蛍光顔料の分散液を、切手用シートの塗被層を形成する
塗被液中に特定量配合することによって、得られた切手
用シートの摩耗度を1000μg以下、好ましくは80
0μg以下に特車するものである。
In the method of the present invention, a specific amount of a dispersion of an inorganic fluorescent pigment that has been subjected to a specific wet pulverization process is blended into a coating liquid that forms the coating layer of a stamp sheet. The wear degree of the sheet is 1000μg or less, preferably 80μg or less.
This is a special vehicle with a concentration of 0 μg or less.

また、印刷適性、即ちグラビア印刷で発生するミスドツ
ト(率)は、下記の方法で評価される。
Furthermore, print suitability, that is, the rate of misdots occurring in gravure printing, is evaluated by the following method.

グラビア印刷適性試験機(大蔵省印刷局方式)を用いて
、試料(如被祇)上にグラビア印刷を施し、網点600
0個当たりの網点の欠損率(ミスドツト率)を求めるも
のである。本発明の方法によって得られた切手用シート
のミスドツト率が10%以下であれば、十分なる印刷品
質が得られる。因みに、10%を越えると印刷効果が不
十分となる。
Using a gravure printing aptitude tester (Ministry of Finance Printing Bureau method), gravure printing was performed on the sample (Nyokai), and the number of halftone dots was 600.
The missing rate (misdot rate) of halftone dots per zero halftone dots is determined. If the misdot rate of the stamp sheet obtained by the method of the present invention is 10% or less, sufficient printing quality can be obtained. Incidentally, if it exceeds 10%, the printing effect will be insufficient.

そして、そのような調整を行うことによって、切手用シ
ートを切手に仕上げる過程で必要な種々の断裁工程にお
けるカッティング刃の磨耗を少なくし、結果的にカッテ
ィング刃の寿命を長くして作業効率を高めるものである
。因に、切手用シトの摩耗度が1000μgを越えると
、カッティング刃の寿命が著しく低下し、製品の切口外
観等が悪くなり、カッティング効率が著しく低下する。
By making such adjustments, wear and tear on the cutting blade during the various cutting processes required in the process of finishing stamp sheets into stamps can be reduced, resulting in longer lifespan of the cutting blade and increased work efficiency. It is something. Incidentally, if the degree of abrasion of the stamp sheet exceeds 1000 μg, the life of the cutting blade will be significantly reduced, the appearance of the cut end of the product will be poor, and the cutting efficiency will be significantly reduced.

前記したように、本発明において塗被層中に用いる無機
蛍光顔料は耐摩耗性、塗工適性(スフランチの抑制)、
或いは経済的(蛍光顔料は高価)な理由から少量が配合
される。従って、その使用に当たっては最大限の発光強
度が得られるように配慮される必要がある。
As mentioned above, the inorganic fluorescent pigment used in the coating layer in the present invention has excellent abrasion resistance, coating suitability (suppression of soufflage),
Alternatively, a small amount is added for economical reasons (fluorescent pigments are expensive). Therefore, when using it, it is necessary to take care to obtain the maximum luminous intensity.

その為に、本発明では該無機蛍光顔料を湿式粉砕し、そ
の粉砕程度を特定するものであるが、これは記述した如
く、■塗工適性の改良、■耐摩耗性を有する塗被紙を得
ること、及び■印刷適性の改善(主にグラビア印刷にお
けるミスドツト率の減少)等を目的とするものである。
Therefore, in the present invention, the inorganic fluorescent pigment is wet-pulverized and the degree of pulverization is determined. and (1) improving printability (mainly reducing the rate of misdots in gravure printing).

ところが、本発明の発光切手用シートについて種々試験
を行って過程で、全(予期しない作用効果の有ることが
判った。
However, during various tests on the luminescent stamp sheet of the present invention, it was found that it had unexpected effects.

即ち、市販の無機蛍光顔料をそのまま湿式粉砕処理を施
さずに、塗被液として調製し、支持体に塗被した後、切
手用シートとして仕上げたものを高湿度の雰囲気中に放
置、又は水中に落とした後に、乾燥してその発光強度を
測定すると、強度(特に印刷後のものについて)が著し
く低下してしまうが、本発明の如く、−度サンドミル等
で特定量の湿式粉砕を施した無機蛍光顔料を用いると、
たとえ高湿度の雰囲気中に晒してもその発光強度が殆ど
低下しないことが明らかとなった。
In other words, a commercially available inorganic fluorescent pigment is prepared as a coating liquid without being wet-pulverized, coated on a support, and then finished as a stamp sheet and left in a high humidity atmosphere or submerged in water. When the luminescence intensity is measured after drying and drying, the intensity (especially after printing) decreases significantly. Using inorganic fluorescent pigments,
It has become clear that the luminescence intensity hardly decreases even when exposed to a high humidity atmosphere.

なお、かくして得られた本発明の切手用シートは、必要
に応して裏面にデキストリン等の水性糊のコーティング
層を設けたり、更に粘着層を介して剥離紙を有する夕、
り切手シートとして仕上げることも可能である。
The thus obtained stamp sheet of the present invention may be coated with a coating layer of an aqueous adhesive such as dextrin on the back side, if necessary, or with a release paper via an adhesive layer.
It is also possible to finish it as a stamp sheet.

以下、実施例を挙げて本発明をより具体的に説明するが
、勿論これらの範囲に限定されるものでない。なお、例
中の「部」及び「%」は、特に断わらない限り、それぞ
れ「重量部」、及び「重量%」を示す。
Hereinafter, the present invention will be explained in more detail with reference to examples, but the present invention is of course not limited to these scopes. Note that "parts" and "%" in the examples indicate "parts by weight" and "% by weight", respectively, unless otherwise specified.

実施例1 無機蛍光顔料(ZnzS ioa:Mn)100部を、
分散剤としてポリアクリル酸ソーダ0.2部を添加した
水中に、固形分濃度が40%の分散液となるようにター
ビン翼型撹拌機を用いて分散した。この分散液をサンド
ミル(回転数80Orpm、流量200j7/H)で処
理した。
Example 1 100 parts of an inorganic fluorescent pigment (ZnzSioa:Mn),
The mixture was dispersed in water to which 0.2 part of sodium polyacrylate was added as a dispersant, using a turbine blade type stirrer, to obtain a dispersion liquid having a solid content concentration of 40%. This dispersion liquid was processed with a sand mill (rotation speed 80 rpm, flow rate 200j7/H).

この時の粉砕前後の比表面積は、Sw、=10000c
m2/ g 、 S wz=8000cm2/ gであ
り、S h + / S w z = 1−25であっ
た。
The specific surface area before and after crushing at this time is Sw, = 10000c
m2/g, S wz = 8000 cm2/g, and S h + / S wz = 1-25.

次に、この分散液5部と、カオリン20部、重質炭酸カ
ルシウム80部、酸化澱粉2部(固形分)、スチレン−
ブタジェン共重合体ラテックス14部(固形分)を混合
し、別に所要の水を添加して固形分濃度58%の塗被液
を得た。
Next, 5 parts of this dispersion, 20 parts of kaolin, 80 parts of heavy calcium carbonate, 2 parts of oxidized starch (solid content), styrene-
14 parts (solid content) of butadiene copolymer latex were mixed, and the required amount of water was separately added to obtain a coating liquid with a solid content concentration of 58%.

この塗被液を64 g/la”の原紙に、絶乾コート量
が20 g/m”となるようにブレードコーターで塗布
し、120℃のドライヤーで乾燥して水分6%の塗被紙
を得た。この塗被紙をスーパーキャレンダー掛けし、更
に裏面にデキストリンを15 gem2(固形分)塗布
して切手用シートを製造した。得られた切手用シートの
評価及び分散液の性質を表に示した。
This coating liquid was applied to 64 g/la" base paper using a blade coater so that the absolute dry coating amount was 20 g/m", and dried with a dryer at 120°C to form a coated paper with a moisture content of 6%. Obtained. This coated paper was super calendered, and 15 gem2 (solid content) of dextrin was further coated on the back side to produce a stamp sheet. The evaluation of the obtained stamp sheet and the properties of the dispersion are shown in the table.

実施例2 無機蛍光顔料としてCaS io3 : pb :Mn
を使用した以外は実施例1と同様にし、得られた分散液
及び切手用シートの評価試験を行い、得られた結果を表
に示した。この時の粉砕前後の比表面積は、Sw+=1
0500 cm”/g 、 Swz=9000cm”/
gであり、Swl/ Swz=1.17であった。
Example 2 CaSio3:pb:Mn as an inorganic fluorescent pigment
An evaluation test was carried out on the obtained dispersion liquid and stamp sheet in the same manner as in Example 1 except that 1 was used, and the obtained results are shown in the table. The specific surface area before and after pulverization at this time is Sw+=1
0500 cm"/g, Swz=9000cm"/
g, and Swl/Swz=1.17.

実施例3 無機蛍光顔料としてZnS : Cuを使用した以外は
実施例1と同様にし、得られた分散液及び切手用シート
の評価試験を行い、得られた結果を表に示した。
Example 3 The procedure of Example 1 was repeated except that ZnS:Cu was used as the inorganic fluorescent pigment, and the obtained dispersion and stamp sheet were evaluated. The results are shown in the table.

この時の粉砕前後の比表面積は、S w+=12500
cm”/g、S町=9000cL1)2/gであり、S
帽/ Swz=1.39であった。
The specific surface area before and after crushing at this time is S w + = 12500
cm”/g, S town=9000cL1)2/g, and S
Hat/Swz=1.39.

比較例1 実施例1において、湿式粉砕処理をしていない無機蛍光
顔料分散液を使用した以外は実施例1と同様Sこし、得
られた分散液及び切手用シートの評価試験を行い、得ら
れた結果を表に示した。
Comparative Example 1 The same procedure as in Example 1 was used except that an inorganic fluorescent pigment dispersion that had not been wet-pulverized was used, and the obtained dispersion and stamp sheet were subjected to an evaluation test. The results are shown in the table.

比較例2 実施例1における無機蛍光顔料分散液をサンドミル(回
転数20Orpm、被分散液流量800j2/H)で処
理した。この時の粉砕前後の比表面積は:SW+281
00 cm2/g 、 Swz=8000cm2/gで
あり、Sw。
Comparative Example 2 The inorganic fluorescent pigment dispersion in Example 1 was treated with a sand mill (rotation speed: 20 rpm, flow rate of liquid to be dispersed: 800 j2/H). The specific surface area before and after crushing at this time is: SW + 281
00 cm2/g, Swz=8000cm2/g, and Sw.

/S−2・1.01であった。それ以外は実施例1と同
様にし、得られた分散液及び切手用シートの評価試験を
行い、得られた結果を表に示した。
/S-2・1.01. Other than that, evaluation tests were conducted on the obtained dispersion liquid and stamp sheet in the same manner as in Example 1, and the obtained results are shown in the table.

比較例3 実施例1における無機蛍光顔料分散液をサンドミル(回
転数200rpm、流量8001/H)で還流処理した
。この時の粉砕前後の比表面積は、Sv、・20000
cm2/g 、 Swz=8000cn2/gであり、
S−1/Swz=2.5であった。それ以外は実施例1
と同様にし、得られた分散液及び切手用シートの評価試
験を行い、得られた結果を表に示した。
Comparative Example 3 The inorganic fluorescent pigment dispersion in Example 1 was refluxed using a sand mill (rotation speed: 200 rpm, flow rate: 8001/H). The specific surface area before and after pulverization at this time is Sv, ・20000
cm2/g, Swz=8000cn2/g,
S-1/Swz=2.5. Other than that, Example 1
Evaluation tests were conducted on the resulting dispersion and stamp sheets in the same manner as above, and the results are shown in the table.

比較例4 実施例1において、湿式粉砕処理した無機蛍光顔料分散
液の添加量を0.5部とした以外は実施例1と同様にし
、得られた分散液及び切手用シートの評価試験を行い、
得られた結果を表に示した。
Comparative Example 4 The procedure of Example 1 was repeated except that the amount of the wet-pulverized inorganic fluorescent pigment dispersion was changed to 0.5 parts, and the obtained dispersion and stamp sheet were evaluated. ,
The results obtained are shown in the table.

比較例5 実施例1において、湿式粉砕処理した無機蛍光顔料分散
液の添加量を12部とした以外は実施例1と同様にし、
得られた分散液及び切手用シートの評価試験を行い、得
られた結果を表に示した。
Comparative Example 5 The same procedure as in Example 1 was carried out except that the amount of the wet-pulverized inorganic fluorescent pigment dispersion was changed to 12 parts,
An evaluation test was conducted on the obtained dispersion liquid and stamp sheet, and the obtained results are shown in the table.

;スクラッチ度〕 : 塗被面に254nmの波長を照射して微細スクラッチの
発生程度を目視判定した。
;Scratch degree]: The coated surface was irradiated with a wavelength of 254 nm, and the degree of occurrence of fine scratches was visually determined.

○発生なし、△微かに発生 ×発生子し 3安定性〕 : 無機蛍光顔料水分散液を湿式粉砕処理後、1日放置した
ときの凝集物(沈降物)の発生度合いを目視判定した。
○ No generation, △ Slight generation × Generation 3 Stability]: After the inorganic fluorescent pigment aqueous dispersion was wet-pulverized, it was left to stand for one day, and the degree of generation of aggregates (sediments) was visually determined.

○凝集物なし、 ×凝集物あり 〔発光強度〕 : (1)−塗被紙に254nmの波長を照射し、励起され
た発光強度(低下の有無) を目視判定した。
○ No aggregates, × Aggregates present [Emission intensity]: (1) - The coated paper was irradiated with a wavelength of 254 nm, and the excited emission intensity (presence or absence of decrease) was visually determined.

○低下なし、 ×低下あり (2)−40℃、90%RH雰囲気下に24時間放置後
、自然乾燥し、254nmの波長 を照射した時の励起発光強度を、上 記処理前のシートと比較してその低 下有無を目視判定した。
○No decrease ×Decrease (2) After being left in an atmosphere of -40°C and 90% RH for 24 hours, it was air-dried and the excitation emission intensity when irradiated with a wavelength of 254 nm was compared with the sheet before the above treatment. The presence or absence of a decrease was visually determined.

○低下なし、 ×低下あり 〔摩耗度〕 : 真鍮針(組成Cu/Zn=52/48 )をミシン(機
械)にセットし、10枚重ねた塗被紙(切手用シート)
に一定条件で続けて10000回穴をあけ(穴は毎回具
なる)、穴あけテストの前後における真鍮針の重量差を
求めて、その値を摩耗度とした(単位:μg)。
○ No deterioration, × Deterioration [Degree of wear]: A brass needle (composition Cu/Zn = 52/48) was set in a sewing machine (machine), and 10 sheets of coated paper (stamp sheet) were stacked.
A hole was continuously drilled under certain conditions 10,000 times (the hole was filled each time), and the difference in weight of the brass needle before and after the hole test was determined, and that value was taken as the degree of wear (unit: μg).

〔ミスドツト率〕 : グラビア印刷適性試験機(大蔵省印刷局方式)にて、グ
ラビア印刷インキを用いて印刷を行い、該印刷物の網点
6000個当たりの欠損率(ミスドツト率)をドツトア
ナライザー(神崎製祇■製開発品)で算出した。
[Miss dot rate]: Printing is performed using gravure printing ink using a gravure printing aptitude tester (Ministry of Finance Printing Bureau method), and the defect rate (misdot rate) per 6000 halftone dots of the printed matter is measured using a dot analyzer (manufactured by Kanzaki). Calculated using a product developed by Gi ■.

(効果) 表に示した本発明の各実施例から明らかなの如く、切手
用シートを構成する塗被層を、特定の;溜弐粉砕処理を
施した無機蛍光顔料の分散液を含有する塗被液で形成す
ると、塗工工程においては勿論、グラビア印刷において
も塗被筋(微細なスクラッチ)が全く発生せず、安定し
た塗工が可能となり、しかもこの切手用シートは、通常
のカッティング刃やダイカット刃に対する摩耗性も著し
く改善されていた。
(Effects) As is clear from the examples of the present invention shown in the table, the coating layer constituting the stamp sheet is a coating containing a dispersion of an inorganic fluorescent pigment that has been subjected to a specific pulverization treatment. When formed with a liquid, there are no coating streaks (fine scratches) during the coating process or gravure printing, and stable coating is possible.Moreover, this stamp sheet can be used with ordinary cutting blades and The abrasion resistance to the die cut blade was also significantly improved.

Claims (6)

【特許請求の範囲】[Claims] (1)支持体上に、顔料、無機蛍光顔料及び接着剤を主
成分とする塗被液を塗被、乾燥して得る切手用シートの
製造方法において、予め、下記条件を満たす比表面積と
なるように無機蛍光顔料を湿式粉砕処理し、処理後の無
機蛍光顔料分散液を塗被液に配合することを特徴とする
切手用シートの製造方法。
(1) In the method for producing stamp sheets obtained by coating a support with a coating liquid containing pigments, inorganic fluorescent pigments, and adhesives as main components and drying, the specific surface area is determined in advance to meet the following conditions. A method for producing a stamp sheet, which comprises wet-pulverizing an inorganic fluorescent pigment and blending the treated inorganic fluorescent pigment dispersion into a coating liquid.
2.0≧Sw_1/Sw_2≧1.05 上記式中、 Sw_1:湿式粉砕処理後の比表面積 Sw_2:湿式粉砕処理前の比表面積 (単位:cm^2/g) (2)無機蛍光顔料の湿式粉砕処理をサンドミルで行う
請求項(1)記載の切手用シートの製造方法。
2.0≧Sw_1/Sw_2≧1.05 In the above formula, Sw_1: Specific surface area after wet pulverization Sw_2: Specific surface area before wet pulverization (unit: cm^2/g) (2) Wet pulverization of inorganic fluorescent pigment The method for producing a stamp sheet according to claim 1, wherein the pulverization treatment is performed using a sand mill.
(3)切手用シートの摩耗度が1000μg以下となる
ように無機蛍光顔料分散液を塗被液に配合する請求項(
1)記載の切手用シートの製造方法。
(3) Claim that the inorganic fluorescent pigment dispersion is blended into the coating liquid so that the degree of abrasion of the stamp sheet is 1000 μg or less (
1) Method for manufacturing the stamp sheet described above.
(4)無機蛍光顔料の配合量が塗被液を構成する全顔料
成分の0.5〜4.0重量%である請求項(3)記載の
切手用シートの製造方法。
(4) The method for producing a stamp sheet according to claim (3), wherein the amount of the inorganic fluorescent pigment blended is 0.5 to 4.0% by weight of the total pigment components constituting the coating liquid.
(5)無機蛍光顔料の配合量が塗被液を構成する全顔料
成分の1.0〜3.0重量%である請求項(4)記載の
切手用シートの製造方法。
(5) The method for producing a stamp sheet according to claim (4), wherein the amount of the inorganic fluorescent pigment is 1.0 to 3.0% by weight of the total pigment components constituting the coating liquid.
(6)グラビア印刷における印刷ミスドット率が10%
以下である請求項(1)〜(5)記載の方法で製造され
た切手用シート。
(6) Printing error dot rate in gravure printing is 10%
A stamp sheet produced by the method according to claims (1) to (5), which is as follows.
JP2324438A 1989-11-27 1990-11-26 Stamp sheet manufacturing method and stamp sheet Expired - Fee Related JP2676712B2 (en)