JPH03250708A - Magnetic recording medium and its manufacture - Google Patents

Magnetic recording medium and its manufacture

Info

Publication number
JPH03250708A
JPH03250708A JP4781790A JP4781790A JPH03250708A JP H03250708 A JPH03250708 A JP H03250708A JP 4781790 A JP4781790 A JP 4781790A JP 4781790 A JP4781790 A JP 4781790A JP H03250708 A JPH03250708 A JP H03250708A
Authority
JP
Japan
Prior art keywords
layer
cobalt
magnetic recording
substrate
ferrite film
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
JP4781790A
Other languages
Japanese (ja)
Inventor
Takashi Ebisawa
孝 海老沢
Hideaki Murata
秀明 村田
Kenichi Sano
謙一 佐野
Junzo Takahashi
高橋 純三
Takaharu Yonemoto
米本 隆治
Tsugio Miyagawa
宮川 亜夫
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
LIMES KK
Original Assignee
LIMES KK
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by LIMES KK filed Critical LIMES KK
Priority to JP4781790A priority Critical patent/JPH03250708A/en
Publication of JPH03250708A publication Critical patent/JPH03250708A/en
Ceased legal-status Critical Current

Abstract

PURPOSE:To improve the crystallinity and magnetic characteristics of a magnetic recording medium by constituting the medium by forming a 43-cobalt layer having a specific thickness between a substrate and cobalt-ferrite film as a base layer. CONSTITUTION:A 43-cobalt layer having a thickness of >=1,500Angstrom is formed between a substrate and cobalt-ferrite film as a base layer. The crystal structure of the 43-cobalt layer (Co3O4 layer) is made to the same spinel type as that of the cobalt ferrite, with their lattice constants close to each other. Moreover, since the Co3O4 layer is formed at a temperature of about 150 deg.C, the layer shows a relatively good crystallinity. Thus, the cobalt-ferrite film is formed on the Co3O4 layer previously formed on a amorphous glass substrate, etc., instead of forming the cobalt-ferrite film directly on the substrate, etc. Therefore, this magnetic recording medium can be improved in crystallinity and magnetic characteristics and reduced in cost.

Description

【発明の詳細な説明】 [産業上の利用分野] 本発明は、磁気記録媒体及びその製造方法に関する。[Detailed description of the invention] [Industrial application field] The present invention relates to a magnetic recording medium and a method for manufacturing the same.

[従来の技術と課題] 近年、酸化物磁性材料を磁気記録媒体としで用いる研究
か多く行われている。ところで、こうした材I)の−っ
であるコバルトフェライトは、薄膜にした場合、イツト
リウム鉄ガーネツト系等に比べて、結晶性が悪く、十分
な磁気特性か15られない。
[Prior Art and Problems] In recent years, many studies have been conducted on the use of oxide magnetic materials as magnetic recording media. By the way, when made into a thin film, cobalt ferrite, which is the material I), has poor crystallinity compared to yttrium iron garnet, etc., and does not have sufficient magnetic properties.

そこで、これらの問題点を解決する手段として、従来、
ガドリニウム・ガリウム・ガーネット(G d 3 G
 3 q O+ 2、GGG)m結晶基板上”\工ビタ
キシャル成長させたり、室温て成膜した後500℃以上
の高温で酸素雰囲気又は大気中で熱処理を行なう等の手
段が講じられていた。しかし、この場合、単結晶基板が
高価であったり、また成膜液高温で熱処理した場合は基
板が耐熱性のものに限られる等の問題点を有する。
Therefore, as a means to solve these problems, conventional
Gadolinium gallium garnet (G d 3 G
Measures have been taken, such as bitaxial growth on a 3q O+ 2, GGG)m crystal substrate, or heat treatment at a high temperature of 500°C or higher in an oxygen atmosphere or the air after forming a film at room temperature. However, in this case, there are problems such as the single crystal substrate is expensive, and if the film forming solution is heat treated at a high temperature, the substrate must be heat resistant.

本発明は上記事情に鑑みてなされたもので、基体とコバ
ルトフェライト膜間に下地層としての厚さ1500Å以
上の四三化コバルト層を介在させることにより、結晶性
及び磁気特性に優れ、かつコスト低減を図ることができ
る磁気記録媒体及びその製造方法を提供することを目的
とする。
The present invention has been made in view of the above circumstances, and by interposing a cobalt tetratriide layer with a thickness of 1500 Å or more as an underlayer between the substrate and the cobalt ferrite film, it has excellent crystallinity and magnetic properties, and is inexpensive. It is an object of the present invention to provide a magnetic recording medium and a method for manufacturing the same that can reduce the amount of noise.

[課題を解決するための手段と作用] 本願第1の発明は、基体と、この基体上に形成された下
地層としての厚さ1500Å以上の四三化コバルト層と
、この四三化コバルト層上に形成されたコバルトフェラ
イト膜とを具備することを特徴とする磁気記録媒体であ
る。
[Means and Effects for Solving the Problems] The first invention of the present application comprises a base, a cobalt tetratriide layer with a thickness of 1500 Å or more as an underlayer formed on the base, and the cobalt tetratriide layer. A magnetic recording medium characterized by comprising a cobalt ferrite film formed thereon.

本願第1の発明によれば、基体とコバルトフェライト膜
間に下地層としての厚さ1500Å以上の四三化コバル
ト層を介した構成とすることにより、結晶性及び磁気特
性を向上できる。
According to the first aspect of the present invention, crystallinity and magnetic properties can be improved by interposing a cobalt tetratriide layer with a thickness of 1500 Å or more as an underlayer between the substrate and the cobalt ferrite film.

本願第2の発明は、基体上に下地層としての厚さ150
0Å以上の四三化コバルト層を形成した後、この四三化
コバルト層上に物理蒸着法によりコノ・ルトフェライト
膜を形成することを特徴とする磁気記録媒体の製造方法
である。
The second invention of the present application provides a base layer with a thickness of 150 mm on the substrate.
This method of manufacturing a magnetic recording medium is characterized in that after forming a cobalt tetratriide layer with a thickness of 0 Å or more, a conorthoferrite film is formed on the cobalt tetratriide layer by physical vapor deposition.

本願第2の発明において、前記四三化コバルト層の形成
手段としては、例えばCoターケ・ントを酸素を含む雰
囲気中でスパッタリングすることが挙げられる。また、
コバルトフェライト膜の形成手段としては、■FeとC
Oを複合ターゲットを酸素を含む雰囲気中でスパッタリ
ングすること、あるいは■■FeターゲットとCOター
ゲ・ソトとを酸素を含む雰囲気中で同時にスバ・ンタリ
ングすること等が挙げられる。
In the second aspect of the present invention, the means for forming the cobalt tetratriide layer may include, for example, sputtering a Co substrate in an atmosphere containing oxygen. Also,
As a means of forming a cobalt ferrite film, ■ Fe and C
Examples include sputtering a composite target with O in an atmosphere containing oxygen, or simultaneously sputtering a Fe target and a CO target in an atmosphere containing oxygen.

本願第1・第2の発明において、四三化コlくルト層(
Co、04層)の厚みを1500Å以上とするのは、次
のような理由による。
In the first and second inventions of the present application, a tetratrichloride melt layer (
The reason why the thickness of the Co, 04 layer) is set to 1500 Å or more is as follows.

下地層としてのCO30a層の結晶構造は、コバルトフ
ェライトのそれと同じでスピネル型であり、格子定数が
近い値をもつ。また、CO3O4層は、150℃程度の
温度で成膜しても比較的良い結晶性を示す。ところで、
膜の結晶成長において、その構造に最も大きく影響する
のは基板材料の結晶構造である。こうしたことから、本
発明者らは、アモルファスのガラス基板等に直接コバル
トフェライト膜を成膜するよりも、上記Co30.、層
を予め基板上に設け、その上にコバルトフェライト膜を
成膜することにより、結晶性が改善され、かつそれに伴
って磁気特性も向上することを究明した。特に、C0,
04層の厚みが1500Å以上のとき本発明効果を発揮
した。
The crystal structure of the CO30a layer as the underlayer is the same as that of cobalt ferrite, which is a spinel type, and the lattice constants have similar values. Further, the CO3O4 layer exhibits relatively good crystallinity even when it is formed at a temperature of about 150°C. by the way,
In the crystal growth of a film, the crystal structure of the substrate material has the greatest influence on its structure. For these reasons, the present inventors decided that the above-mentioned Co30. discovered that by providing a layer on a substrate in advance and depositing a cobalt ferrite film on it, the crystallinity was improved and the magnetic properties were improved accordingly. In particular, C0,
The effect of the present invention was exhibited when the thickness of the 04 layer was 1500 Å or more.

上記00304層及びコバルトフェライト膜の成膜法と
しては、上記スパッタリング法の他、■タングステンの
ワイヤーやボードを抵抗加熱して材料を蒸発させるもの
や、電子ビームを材料に当てることで加熱して蒸発させ
るもの等、真空蒸着法を酸素を含む雰囲気中で行う物理
的成膜法、■上記酸素や蒸発原子を高周波コイルや電子
線によりイオン化して反応性を高めて成膜するイオンブ
レーティング法、 ■蒸発原子にイオンガンより酸素イオンを照射しつつ成
膜するイオンアシスト法、 等があり、これらの成膜法を用いてもCogO4層及び
コバルトフェライト膜を容易に成膜でき、特に特定の成
膜法に限定されない。しかし、成膜の安定性、膜の結晶
性、操作性などを考慮すれば、スパッタリング法か最も
有利である。中でも、FeまたはCO夕−ケラト上にC
OまたはFeのチップ又はタブレットを乗せた複合ター
ゲットを用いた場合、そのチップ又はタブレットの形状
や個数を変えることで組成を自由に変えることができ、
合金ターゲットや複数のターゲットを用いるよりもコス
ト的に安くなる。また、FeとCoのターゲットを同時
にスパッタリングした場合も、■2つのターゲットを用
いるので成膜速度を速くてき、■その成膜速度はスパッ
タ電力を変える事で制御できることから、膜の組成も自
由に制御でき、■下地層としての60304層を同一バ
ッチ内で成膜できる、という利点を有する。
In addition to the above-mentioned sputtering method, methods for forming the 00304 layer and cobalt ferrite film include: 1) heating a tungsten wire or board to evaporate the material, and heating and evaporating the material by exposing it to an electron beam. physical film forming method in which the vacuum evaporation method is performed in an atmosphere containing oxygen; ■ ion blating method in which the oxygen and evaporated atoms are ionized using a high frequency coil or electron beam to increase reactivity and form a film; ■Ion-assist method, which forms a film while irradiating evaporated atoms with oxygen ions from an ion gun, etc. These film-forming methods can also be used to easily form a CogO4 layer and a cobalt ferrite film. Not limited to law. However, considering the stability of film formation, crystallinity of the film, operability, etc., the sputtering method is the most advantageous. Among them, Fe or CO2-C on the kerato
When using a composite target loaded with O or Fe chips or tablets, the composition can be freely changed by changing the shape and number of the chips or tablets.
It is cheaper in cost than using an alloy target or multiple targets. Also, when sputtering Fe and Co targets at the same time, the film formation rate can be increased because two targets are used, and the film composition can be controlled freely by changing the sputtering power. It has the advantage that 60304 layers as an underlayer can be formed in the same batch.

第2図(A)、(B)は、本発明に係るマグネトロンス
パッタ装置の説明図であり、同図(A)は正面図、同図
(B)は同図(A)の部分平面図である。
FIGS. 2(A) and 2(B) are explanatory views of the magnetron sputtering apparatus according to the present invention; FIG. 2(A) is a front view, and FIG. 2(B) is a partial plan view of FIG. 2(A). be.

図中の1は真空チャンバーである。この真空チャンバー
1内の下部には、上部にターゲット2を載置したカソー
ド3か、複数個仕切板4を介して配置されている。前記
真空チャンバー1内の上部には、基板5を把持する基板
ホルダー6が設けられている。前記真空チャンバー1の
所定の位置には、スパッタガスの導入管7、排気管8が
夫々設けられている。
1 in the figure is a vacuum chamber. In the lower part of the vacuum chamber 1, a plurality of cathodes 3, each having a target 2 mounted thereon, are arranged via a partition plate 4. A substrate holder 6 for holding the substrate 5 is provided at the upper part of the vacuum chamber 1 . A sputtering gas introduction pipe 7 and an exhaust pipe 8 are provided at predetermined positions in the vacuum chamber 1, respectively.

以下、本発明の実施例について比較例とともに説明する
。
Examples of the present invention will be described below along with comparative examples.

[実施例1コ 本実施例1では、ターゲットとして、Feターゲット上
に直径10I111%厚さ5mmのCOタブレットを5
ヶ乗せた複合ターゲットと、Coターゲットを用いる。
[Example 1] In this Example 1, 5 CO tablets with a diameter of 10I111% and a thickness of 5 mm were placed on an Fe target as a target.
A composite target and a Co target are used.

又、基板としては、ガラス基板(商品名:コーニング7
059、コーニング社製)を用いた。
In addition, as a substrate, a glass substrate (product name: Corning 7
059, manufactured by Corning Inc.) was used.

■CO3O4層の形成 まず、前記ガラス基板上に、下記条件でDCマグネトロ
ンスパッタ法により反応性スパッタリングを行い、Co
ターゲットのみを用いて厚さ3000人の00304層
を堆積した。
■Formation of CO3O4 layer First, reactive sputtering was performed on the glass substrate by DC magnetron sputtering under the following conditions.
A 3000 layer thick 00304 layer was deposited using only the target.

スパッタガス :Ar+02 スパッタガス圧: 5mTorr  (409002)
スパッタ電流 :2A 基板温度   :室温 この結果、得られた薄膜は、X線回折により(311)
面に優先配向したCO3O4層であり、常温で強磁性を
示さなかった。
Sputter gas: Ar+02 Sputter gas pressure: 5 mTorr (409002)
Sputtering current: 2A Substrate temperature: Room temperature As a result, the obtained thin film was determined by X-ray diffraction (311)
It was a CO3O4 layer with preferential orientation in the plane, and did not exhibit ferromagnetism at room temperature.

■コバルトフェライト膜の形成 次に、前記複合ターゲットのみを用いて、前記CO3O
4層上3に、下記条件てDCマグネトロンスバッ法によ
り反応性スパッタリングを行い、厚さ2000人のコバ
ルトフェライト膜を形成した。
■ Formation of cobalt ferrite film Next, using only the composite target, the CO3O
Reactive sputtering was performed on the fourth layer 3 by the DC magnetron sputtering method under the following conditions to form a cobalt ferrite film with a thickness of 2000 mm.

スパッタガス :Ar+02 スパッタガス圧:5mTorr  (40%O2)スパ
ッタ電流 =2A 基板温度   :400℃ この結果、得られた薄膜の磁気特性は、磁化M −12
7emu/ cm3(IOK Oe :以下すべての磁
化、保磁力はIOK Oeの磁界中での値である)、保
磁力Hc −11,000e (以下全ての保磁力は面
内方向である)であった。
Sputtering gas: Ar+02 Sputtering gas pressure: 5mTorr (40% O2) Sputtering current = 2A Substrate temperature: 400°C As a result, the magnetic properties of the obtained thin film are as follows: magnetization M -12
7 emu/cm3 (IOK Oe: All magnetization and coercive force below are values in the magnetic field of IOK Oe), coercive force Hc -11,000e (all coercive forces below are in the in-plane direction). .

[比較例1] 本比較例1では、実施例1と比べ、00304層の成膜
かない以外同様の条件でコバルトフェライト膜を作製し
た。この結果、得られた薄膜は、X線回折により(31
1)面に優先配向したコバルトフェライト膜であり、そ
の磁気特性は磁化M−110emu/ c+a3、保磁
力Hc−9400eてあった。
[Comparative Example 1] In Comparative Example 1, a cobalt ferrite film was produced under the same conditions as in Example 1 except that the 00304 layer was not formed. As a result, the obtained thin film was analyzed by X-ray diffraction (31
1) It was a cobalt ferrite film preferentially oriented in the plane, and its magnetic properties were a magnetization of M-110emu/c+a3 and a coercive force of Hc-9400e.

上記実施例1と比較例1より、Co3O4層を下地層と
した場合に磁気特性を改善する方向に導くことが分かる
。また、00304層の厚さを変えて同様の実験を行っ
たところ、膜の磁気特性は第1図に示すような変化を示
した。このことから、Co3O4層を設けてコバルトフ
ェライト膜の磁気特性を向上させるには、CO3O4層
の厚さを少なくとも1500Å以上にする必要があるこ
とが分かる。
From the above Example 1 and Comparative Example 1, it can be seen that the magnetic properties are improved when the Co3O4 layer is used as the underlayer. Furthermore, when similar experiments were carried out by changing the thickness of the 00304 layer, the magnetic properties of the film showed changes as shown in FIG. From this, it can be seen that in order to improve the magnetic properties of the cobalt ferrite film by providing the Co3O4 layer, the thickness of the CO3O4 layer must be at least 1500 Å or more.

[実施例2] 本実施例2ては、Co30.層の作製の際、基板温度を
400℃とした以外は全て実施例1と同様に行った。こ
の結果、得られたCO3O4層は(111)面に強い配
向性を示し、回折強度も大きくなった。
[Example 2] In this example 2, Co30. The layers were prepared in the same manner as in Example 1 except that the substrate temperature was 400°C. As a result, the obtained CO3O4 layer exhibited strong orientation in the (111) plane, and the diffraction intensity also increased.

次に、前記CO3O4層上に、実施例1と同様、コバル
トフェライト膜を形成した。この結果、得られた薄膜の
磁気特性は、磁化M −144emu/ cn’保磁力
Hc −1,6150eであり、実施例1より更に改善
されていることか明らかであった。これにより、003
04層の配向性や結晶性か磁気特性に関与していること
か明らかである。
Next, a cobalt ferrite film was formed on the CO3O4 layer in the same manner as in Example 1. As a result, the magnetic properties of the obtained thin film were magnetization M -144emu/cn' coercive force Hc -1,6150e, and it was clear that the magnetic properties were further improved from Example 1. As a result, 003
It is clear that the orientation and crystallinity of the 04 layer are involved in the magnetic properties.

なお、実施例2でCO3O4層の作製温度を400℃と
したのはコバルトフェライト膜の作製温度か400℃で
あるからであり、150℃程度の温度でも(11,1)
面配向のCo、04層を得ることがてきる。
In addition, the reason why the production temperature of the CO3O4 layer was set at 400°C in Example 2 is because the production temperature of the cobalt ferrite film is 400°C, and even at a temperature of about 150°C (11, 1)
A plane-oriented Co,04 layer can be obtained.

[実施例3] 本実施例3ては、第2図図示の装置にFeとCoのター
ゲットを配置した。
[Example 3] In Example 3, Fe and Co targets were placed in the apparatus shown in FIG.

まず、実施例1と同様00304層を作製した後、Fe
とCoターゲットを用いて下記の条件でDCマグネトロ
ンスパッタリング法により反応性スパッタリングを行い
、厚さ2000人のコバルトフェライト膜を堆積した。
First, as in Example 1, a 00304 layer was prepared, and then Fe
Reactive sputtering was performed by DC magnetron sputtering using a Co target and a Co target under the following conditions to deposit a cobalt ferrite film with a thickness of 2000 mm.

スパッタガス  A r +Q2 スパッタガス圧: 5mTorr  (40%0□)ス
パッタ電流 :2A(Feターゲット)IA(Coター
ゲット) 基板温度   、400℃ 二の結果、得られた薄膜の磁気特性は、磁化M −12
5erAu/cm’ 、保磁力Hc −1,0500e
であった。
Sputtering gas A r +Q2 Sputtering gas pressure: 5mTorr (40%0□) Sputtering current: 2A (Fe target) IA (Co target) Substrate temperature: 400°C As a result of the above, the magnetic properties of the obtained thin film are as follows: Magnetization M − 12
5erAu/cm', coercive force Hc -1,0500e
Met.

[発明の効果] 以上詳述した如く本発明によれば、結晶性及び磁気特性
に優れ、かつコスト低減を図ることができる信頼性の高
い磁気記録媒体及びその製造方法を提供できる。
[Effects of the Invention] As described in detail above, according to the present invention, it is possible to provide a highly reliable magnetic recording medium that has excellent crystallinity and magnetic properties and can reduce costs, and a method for manufacturing the same.

【図面の簡単な説明】[Brief explanation of drawings]

第1図は本発明に係るコバルトフェライト膜の磁気特性
図、第2図は本発明に係るマグネトロンスパッタ装置の
説明図である。
FIG. 1 is a magnetic characteristic diagram of a cobalt ferrite film according to the present invention, and FIG. 2 is an explanatory diagram of a magnetron sputtering apparatus according to the present invention.

Claims (5)

【特許請求の範囲】[Claims] (1)基体と、この基体上に形成された下地層としての
厚さ1500Å以上の四三化コバルト層と、この四三化
コバルト層上に形成されたコバルトフェライト膜とを具
備することを特徴とする磁気記録媒体。
(1) It is characterized by comprising a base, a cobalt tetratriide layer with a thickness of 1500 Å or more as an underlayer formed on the base, and a cobalt ferrite film formed on the cobalt tetratriide layer. magnetic recording media.
(2)基体上に下地層としての厚さ1500Å以上の四
三化コバルト層を形成した後、この四三化コバルト層上
に物理蒸着法によりコバルトフェライト膜を形成するこ
とを特徴とする磁気記録媒体の製造方法。
(2) Magnetic recording characterized by forming a cobalt tetratriide layer with a thickness of 1500 Å or more as an underlayer on a substrate, and then forming a cobalt ferrite film on the cobalt tetratriide layer by physical vapor deposition. Method of manufacturing media.
(3)前記四三化コバルト層か、Coターゲットを酸素
を含む雰囲気中でスパッタリングすることにより形成さ
れる請求項2記載の磁気記録媒体の製造方法。
(3) The method for manufacturing a magnetic recording medium according to claim 2, wherein the cobalt tetratride layer is formed by sputtering a Co target in an atmosphere containing oxygen.
(4)前記コバルトフェライト膜が、FeとCoの複合
ターゲットを酸素を含む雰囲気中でスパッタリングする
ことにより形成される請求項2記載の磁気記録媒体の製
造方法。
(4) The method of manufacturing a magnetic recording medium according to claim 2, wherein the cobalt ferrite film is formed by sputtering a composite target of Fe and Co in an atmosphere containing oxygen.
(5)前記コバルトフェライト膜が、Feターゲットと
Coターゲットとを酸素を含む雰囲気中で同時にスパッ
タリングすることにより形成される請求項2記載の磁気
記録媒体の製造方法。
(5) The method of manufacturing a magnetic recording medium according to claim 2, wherein the cobalt ferrite film is formed by simultaneously sputtering an Fe target and a Co target in an atmosphere containing oxygen.
JP4781790A 1990-02-28 1990-02-28 Magnetic recording medium and its manufacture Ceased JPH03250708A (en)