JPH0328054B2 - - Google Patents
Info
- Publication number
- JPH0328054B2 JPH0328054B2 JP55143356A JP14335680A JPH0328054B2 JP H0328054 B2 JPH0328054 B2 JP H0328054B2 JP 55143356 A JP55143356 A JP 55143356A JP 14335680 A JP14335680 A JP 14335680A JP H0328054 B2 JPH0328054 B2 JP H0328054B2
- Authority
- JP
- Japan
- Prior art keywords
- hcl
- gas
- growth
- region
- gaas
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Lifetime
Abstract
Description
【発明の詳細な説明】
本発明は−族化合物半導体と−族化合
物混晶半導体のハロゲン気相成長法に係るもの
で、特にエピタキシヤル成長層の再現性の向上に
関するものである。DETAILED DESCRIPTION OF THE INVENTION The present invention relates to a halogen vapor phase growth method for -group compound semiconductors and -group compound mixed crystal semiconductors, and particularly relates to improving the reproducibility of epitaxially grown layers.
−族化合物半導体および−族化合物混
晶半導体はマイクロ波デバイスやオプトエレクト
ロニクスデバイス用の材料として重要さを増して
いる。これらの材料は結晶基板の上に液相成長あ
るいは気相成長によつてエピタキシヤル成長され
るが、その成長法は、デバイス作成の上で障害と
ならぬ様に、成長速度や結晶組成、不純物濃度な
どの各パラメータを再現性よく実現できるもので
なければならない。 - Group compound semiconductors and - group compound mixed crystal semiconductors are becoming increasingly important as materials for microwave devices and optoelectronic devices. These materials are grown epitaxially on a crystal substrate by liquid phase growth or vapor phase growth, but the growth method is carefully controlled to ensure growth speed, crystal composition, impurities, etc., so as not to interfere with device fabrication. It must be possible to realize each parameter such as concentration with good reproducibility.
−族化合物半導体あるいは−族化合物
混晶半導体のハロゲン気相成長法にはAsCl3等の
ハロゲン化合物を用いるハライド法と呼ばれる方
法と、AsH3等の水素化合物を用いるハイドライ
ド法と呼ばれる方法の2つの方法がある。ハライ
ド法では、基板結晶付近あるいはこの上流部分の
反応管内壁への結晶の析出がほとんど見られない
ため、成長速度やドーピング特性の再現性の点か
らは有利である反面、原料部での反応が不安定と
なりやすいため、結局は再現性の低下を招く欠点
がある。一方、族元素を水素化物として反応管
内に導入するハイドライド法は原料部での族金
属とHCl等のハロゲンガスとの反応が非常に安定
であり、この成長方法は単に2元の−化合物
半導体の気相成長だけでなく、3元あるいは4元
の−化合物混晶半導体の様な組成制御を必要
とする気相成長において不可欠な方法である。し
かし、ハイドライド法では基板結晶付近あるいは
この上流部分の反応管内壁への結晶の析出がたび
たび発生するが、その析出量が一定でないため成
長速度の再現性を悪化させる。さらに、成長速度
が時間依存性を持つために、成長の制御が困難と
なる。この様な反応管内壁への結晶の析出は−
族化合物混晶半導体を気相成長させる場合には
更に深刻な問題となる。反応管内壁への結晶の析
出は原料ガスの枯渇をもたらすため原料ガス成分
あるいは成分比を変化させるために成長させた混
晶半導体の組成を目的の値とずれたものにしてし
まう。 There are two methods of halogen vapor phase growth for -group compound semiconductors or -group compound mixed crystal semiconductors: the halide method, which uses a halogen compound such as AsCl 3 , and the hydride method, which uses a hydrogen compound such as AsH3 . There is a way. In the halide method, precipitation of crystals near the substrate crystal or on the inner wall of the reaction tube in the upstream part is advantageous in terms of growth rate and reproducibility of doping characteristics. Since it tends to become unstable, it has the disadvantage of ultimately leading to a decrease in reproducibility. On the other hand, in the hydride method, in which a group element is introduced into the reaction tube as a hydride, the reaction between the group metal and a halogen gas such as HCl in the raw material is very stable, and this growth method simply produces a binary compound semiconductor. This is an indispensable method not only for vapor phase growth but also for vapor phase growth that requires composition control, such as in the case of ternary or quaternary compound mixed crystal semiconductors. However, in the hydride method, crystals often precipitate near the substrate crystal or on the inner wall of the reaction tube upstream thereof, but the amount of crystal precipitated is not constant, which deteriorates the reproducibility of the growth rate. Furthermore, since the growth rate is time-dependent, it is difficult to control the growth. This kind of precipitation of crystals on the inner wall of the reaction tube is -
This problem becomes even more serious when a group compound mixed crystal semiconductor is grown in a vapor phase. Precipitation of crystals on the inner wall of the reaction tube leads to depletion of the raw material gas, so that the composition of the mixed crystal semiconductor grown to change the raw material gas components or component ratios deviates from the desired value.
本発明の目的は−族化合物半導体あるいは
−族化合物混晶半導体のハイドライド法にお
ける従来の欠点を除去して、反応管内壁への結晶
の析出がなく、エピタキシヤル成長層の成長速度
の再現性が良く、混晶半導体の成長に対しては混
晶組成の再現性の良いハイドライド法による−
族化合物半導体の気相成長法を提供することに
ある。 The purpose of the present invention is to eliminate the conventional drawbacks of the hydride method for -group compound semiconductors or -group compound mixed crystal semiconductors, eliminate the precipitation of crystals on the inner wall of the reaction tube, and improve the reproducibility of the growth rate of the epitaxial growth layer. For the growth of mixed crystal semiconductors, the hydride method has good reproducibility of the mixed crystal composition.
An object of the present invention is to provide a method for vapor phase growth of group compound semiconductors.
本発明によれば−族化合物半導体のハイド
ライド法ハロゲン気相成長装置において、族元
素ハライドと族元素ハイドライドの混合領域、
あるいはこの下流かつ基板上流の領域に、ハロゲ
ンガス、ハロゲン化水素あるいは族元素ハライ
ドを導入することを特徴とする−族化合物半
導体の気相成長法が得られる。 According to the present invention, in the hydride method halogen vapor phase growth apparatus for -group compound semiconductor, a mixed region of group element halide and group element hydride;
Alternatively, a method for vapor phase growth of - group compound semiconductors can be obtained, which is characterized in that halogen gas, hydrogen halide, or group element halide is introduced into the downstream region and upstream of the substrate.
以下本発明について−族化合物半導体のひ
とつであるGaAsを取上げて詳しく説明する。 The present invention will be explained in detail below by taking up GaAs, which is one of the - group compound semiconductors.
GaAsのハライド法であるAsCl3(三塩化砒素)
法では第1図の様にAsCl3の導入管1より導入さ
れたAsCl3は
AsCl3+3/2H2=1/4As4+3HCl (1)
なる化学式に従つてH2と反応しAs4とHClとに分
解される。発生したHClはT1に保たれた原料領
域で、原料GaAs2と反応し、
GaCl+1/4As4+1/2H2=GaAs+HCl (2)
なる化学反応を左向きに進行させ、平衡状態とな
る。すなわち、HClはGaAsと反応してGaClと
As4を発生させる。これらのガスは温度T1での平
衡分圧のままT1より低い温度T2に保たれた下流
の成長領域3へ輸送され、基板結晶4上において
(2)の化学反応が右向きに進行し、基板結晶上に
GaAsがエピタキシヤル成長する。すなわち、基
板結晶と接触する原料ガス中のGaClとAs4は反応
してGaAsを基板結晶上に析出し、発生したHCl
ガスは基板表面から離脱し、下流に廃出される。
もし、原料のGaAsと基板結晶の間の反応管内壁
5上で(2)の化学反応が右向きに進行してGaAsが
析出すれば、原料ガス中のGaCl成分とAs4成分が
少なくなり、基板結晶上の成長速度は小さくなつ
て再現性が悪くなるばかりか成長速度が時間依存
性を持つようになる。しかし、現実にはAsCl3法
におけるGaAsの成長では、標準的に用いられる
成長条件であるT1=850℃、T2=750℃、PAsC13゜
=3×10-3atmにおいては反応管内壁への結晶の
析出は殆んど無く、再現性の良いエピタキシヤル
成長を行なうことができる。 AsCl 3 (arsenic trichloride) which is a halide method for GaAs
In the method, as shown in Figure 1, AsCl 3 introduced from the AsCl 3 introduction pipe 1 reacts with H 2 according to the chemical formula AsCl 3 + 3/2H 2 = 1/4 As 4 + 3HCl (1) to form As 4 and HCl . It is decomposed into. The generated HCl reacts with the raw material GaAs 2 in the raw material region maintained at T 1 , causing the chemical reaction GaCl+1/4As 4 +1/2H 2 =GaAs+HCl (2) to proceed to the left, resulting in an equilibrium state. In other words, HCl reacts with GaAs to form GaCl.
Generate As 4 . These gases are transported to the downstream growth region 3 maintained at a temperature T 2 lower than T 1 while maintaining their equilibrium partial pressure at the temperature T 1 , and are deposited on the substrate crystal 4 .
The chemical reaction in (2) progresses to the right, and the chemical reaction in
GaAs grows epitaxially. In other words, GaCl and As 4 in the source gas that comes into contact with the substrate crystal react to precipitate GaAs on the substrate crystal, and the generated HCl
The gas leaves the substrate surface and is exhausted downstream.
If the chemical reaction (2) progresses to the right on the inner wall 5 of the reaction tube between the raw material GaAs and the substrate crystal, and GaAs is precipitated, the GaCl component and As 4 component in the raw material gas will decrease, and the substrate Not only does the growth rate on the crystal decrease and reproducibility deteriorate, but the growth rate also becomes time-dependent. However, in reality, in the growth of GaAs using the AsCl 3 method, under the standard growth conditions of T 1 = 850°C, T 2 = 750°C, P AsC13 ° = 3 × 10 -3 atm, the inner wall of the reaction tube There is almost no crystal precipitation, and epitaxial growth can be performed with good reproducibility.
GaAsをハイドライド法であるAsH3(アルシ
ン)法によつて成長する場合には第2図の様に上
流には原料金属Ga6が置かれる。金属GaはHCl導
入管7より導入されたHClと
Ga+HCl=GaCl+1/2H2 (3)
なる化学反応によつてGaClガスを発生する。こ
の反応は平衡論的にほぼ100%で右方に進行する。
すなわち、導入されたHClガスは、そのほとんど
全部がGaClに変換される。発生したGaClは混合
領域8に輸送され、バイパス管9より導入された
AsH3ガスと混合される。AsH3は分解しやすく、
ここで
AsH3=1/4As4+3/2H2 (4)
なる反応によつてAs4とH2とに分解される。
GaClとAs4の混合ガスは更に下流の基板結晶4上
に輸送され、AsCl3法による成長と同じく、(2)の
化学反応によつて基板結晶上にGaAsをエピタキ
シヤル成長させる。しかしAsH3法はAsCl3法と
は異なり、混合領域から基板結晶までの反応管内
壁10上にGaAsの結晶が析出し、基板結晶に接
触する原料ガス中のGaCl、As4濃度がこの析出と
ともに時間的に変化し、そのため成長速度が時間
に依存し、エピタキシヤル成長膜の再現性が悪
い。 When GaAs is grown by the AsH 3 (arsine) method, which is a hydride method, a raw material metal Ga 6 is placed upstream as shown in FIG. Metal Ga generates GaCl gas through a chemical reaction with HCl introduced from the HCl introduction pipe 7: Ga+HCl=GaCl+1/2H 2 (3). This reaction progresses to the right almost 100% of the time in equilibrium.
That is, almost all of the introduced HCl gas is converted to GaCl. The generated GaCl was transported to the mixing region 8 and introduced through the bypass pipe 9.
Mixed with AsH3 gas. AsH 3 is easy to decompose;
Here, AsH 3 =1/4As 4 +3/2H 2 (4) is decomposed into As 4 and H 2 by the reaction.
The mixed gas of GaCl and As 4 is transported further downstream onto the substrate crystal 4, and GaAs is epitaxially grown on the substrate crystal by the chemical reaction (2), similar to the growth by the AsCl 3 method. However, the AsH 3 method differs from the AsCl 3 method in that GaAs crystals are precipitated on the inner wall 10 of the reaction tube from the mixing region to the substrate crystal, and the GaCl and As 4 concentrations in the source gas that come into contact with the substrate crystal are reduced along with this precipitation. The growth rate is time dependent and the reproducibility of epitaxially grown films is poor.
AsCl3法においてもAsH3法においても、成長
反応の化学反応式は(2)式であつて全く同じである
のに、上で説明した様な差の生ずる原因につい
て、以下に−化合物半導体のひとつとして
GaAsを取上げ、反応管内壁への結晶の析出のメ
カニズムを詳しく説明する。 Although the chemical reaction formula for the growth reaction is Equation (2) and is exactly the same in both the AsCl 3 method and the AsH 3 method, the reason for the difference as explained above is explained below. as one
We will focus on GaAs and explain in detail the mechanism of crystal precipitation on the inner wall of the reaction tube.
球状あるいはおわん状の結晶3次元核が気相中
で発生する問題は3次元核形成問題としてよく知
られている。3次元核の生成自由エネルギー△G
は
△G=△Gsurface+△Gbulk (5)
として表わされる。すなわち、3次元核の生成自
由エネルギーは核の表面エネルギーの寄与△
Gsurfaceと体積エネルギーの寄与△Gbulkの和と
して表わされる。表面エネルギー△Gsurfaceは
結晶の表面を作り出すために必要なエネルギーで
あるから、基本的には原子間の結合を切断するに
要するエネルギーであつて、必ず正の符号を持
つ。もちろん、反応式(2)で成長する場合、結晶の
表面は各種の吸着原子あるいは吸着分子のため
に、理想的に清浄な場合に期待される表面エネル
ギー密度とは異なる値になつているが、その符号
が正であることに変わりはない。3次元核が反応
管内壁に成長する場合△Gsurfaceは表面エネル
ギーの他に、反応管と結晶との界面エネルギーを
含む式とならねばならない。いずれの場合におい
ても、3次元核の半径をγとすれば、△
Gsurfaceはγの2乗に比例する量である。すな
わち
△Gsurface=A・γ2 (6)
と書くことができる。 The problem in which spherical or bowl-shaped three-dimensional crystal nuclei occur in the gas phase is well known as the three-dimensional nucleation problem. Free energy of formation of three-dimensional nucleus △G
is expressed as △G=△Gsurface+△Gbulk (5). In other words, the free energy of formation of a three-dimensional nucleus is the contribution of the surface energy of the nucleus △
It is expressed as the sum of Gsurface and volume energy contribution △Gbulk. Since surface energy ΔGsurface is the energy required to create the surface of a crystal, it is basically the energy required to break bonds between atoms, and always has a positive sign. Of course, when growing according to reaction formula (2), the surface energy density of the crystal differs from the surface energy density expected in an ideally clean case due to various adatoms or adsorbed molecules. The sign remains positive. When a three-dimensional nucleus grows on the inner wall of a reaction tube, ΔGsurface must be an expression that includes the interfacial energy between the reaction tube and the crystal in addition to the surface energy. In either case, if the radius of the three-dimensional nucleus is γ, then △
Gsurface is a quantity proportional to the square of γ. That is, it can be written as △Gsurface=A・γ 2 (6).
体積エネルギー△Gbulkは固相1molの析出に
よる熱力学的な自由エネルギー変化量△Gvに3
次元核の体積をかけたものである。従つて△
Gbulkはγ3に比例した量である。すなわち
△Gbulk=B・△Gv・γ3 (7)
となる。従つて3次元核の生成自由エネルギーは
△G=Aγ2+B△Gvγ3 (8)
となる。 The volume energy △Gbulk is calculated by adding 3 to the thermodynamic free energy change △Gv due to the precipitation of 1 mol of solid phase.
It is multiplied by the volume of the dimensional nucleus. Therefore △
Gbulk is a quantity proportional to γ3 . In other words, △Gbulk=B・△Gv・γ 3 (7). Therefore, the free energy of formation of a three-dimensional nucleus is △G=Aγ 2 +B△Gvγ 3 (8).
△Gvは気相が過飽和であれば負の値、未飽和
であれば正の値である。△Gv<0のとき(8)式は
第3図に図示する様に臨界核径γ*において△G
が最大値△G*を持つ。γ*より小さな核は消滅し
ようとし、γ*より大きな核は成長しようとする。
従つて反応管内壁への成長を抑制するためには△
Gvを負ではあるが絶対値の小さな値となるよう
に成長条件を選べばγ*および△G*を大きな値と
することができ、3次元核の形成のためには大き
なエネルギーバリヤ△G*を起えなければならな
くなるので、3次元核発生の確率は小さくなり、
目的が達せられることになる。 ΔGv is a negative value if the gas phase is supersaturated, and a positive value if it is unsaturated. When △Gv<0, equation (8) is expressed as △G at the critical nuclear diameter γ * , as shown in Figure 3.
has the maximum value △G * . Nuclei smaller than γ * tend to disappear, and nuclei larger than γ * tend to grow.
Therefore, in order to suppress the growth on the inner wall of the reaction tube, △
If the growth conditions are chosen so that Gv is negative but small in absolute value, γ * and △G * can be made large values, and a large energy barrier △G * is required for the formation of three-dimensional nuclei. has to occur, the probability of three-dimensional nucleation becomes smaller,
The purpose will be achieved.
基板結晶上への成長は上で説明した3次元核の
形成とは全く異なるメカニズムによつて、△Gv
が負ではあるが絶対値の小さな場合でも起こるた
め、3次元核が反応管内壁に析出しない条件で基
板結晶上にGaAsをエピタキシヤル成長させるこ
とが可能である。以下に基板結晶への成長につい
て説明する。 The growth on the substrate crystal is caused by a completely different mechanism from the three-dimensional nucleus formation explained above.
Although negative, this occurs even when the absolute value is small, so it is possible to epitaxially grow GaAs on the substrate crystal under conditions that three-dimensional nuclei do not precipitate on the inner wall of the reaction tube. The growth on the substrate crystal will be explained below.
基板結晶上にエピタキシヤル成長するときに
は、新しく成長した層は古いGaAs表面を消滅さ
せ、その替り成長層の厚さだけ離れた場所に消滅
した面積と同じ面積の新しいGaAs表面を作り出
す。従つてエピタキシヤル成長による表面エネル
ギーの増加は無い。ところが体積が増加している
ために体積エネルギーは変化している。しかも、
結晶表面にはらせん転位などによつて供給され続
けるステツプやキンクが有るために、表面をミク
ロに見ればこれらが結晶の成長点となり、成長の
バリヤを極めて小さくする原因となつている。従
つて、わずかでも過飽和のある場合には基板結晶
上にエピタキシヤル成長が起こる。 When grown epitaxially on a substrate crystal, the newly grown layer annihilates the old GaAs surface and replaces it with a new GaAs surface with the same area as the annihilated area, separated by the thickness of the grown layer. Therefore, there is no increase in surface energy due to epitaxial growth. However, because the volume is increasing, the volumetric energy is changing. Moreover,
Since there are steps and kinks on the crystal surface that are continuously supplied by screw dislocations, etc., when looking at the surface microscopically, these become crystal growth points and are the cause of extremely small growth barriers. Therefore, if there is even a slight supersaturation, epitaxial growth will occur on the substrate crystal.
次に△Gvについて詳しく説明する。△Gvは
1molの固相が析出した時の系の自由エネルギー
変化であるから、例えば水蒸気からの水滴の成長
の場合には
△Gv=−RT ln(p/pe (9)
である。ここでRはガス定数、Tは絶対温度、p
は水蒸気の分圧、peは水蒸気の平衡分圧である。 Next, △Gv will be explained in detail. △Gv is
Since this is the free energy change of the system when 1 mol of solid phase is precipitated, for example, in the case of the growth of water droplets from water vapor, △Gv=-RT ln(p/p e (9). Here, R is gas constant, T is absolute temperature, p
is the partial pressure of water vapor, and p e is the equilibrium partial pressure of water vapor.
(9)式は水の化学ポテンシヤル変化を考慮するこ
とによつて理解できる。水蒸気から水滴が成長す
る反応を化学式で書けば
H2O(g)=H2O(l) (10)
となる。gはガス、lは液体状態であることを表
わしている。水蒸気の平衡分圧がPe、実際の水
蒸気圧がPとする。水滴の近傍で熱平衡が成立し
ていれば
μe(g)=μ(l) (11)
である。ここでμe(g)は気相中の水蒸気の熱平衡
における化学ポテンシヤル、μ(l)は水滴中の化学
ポテンシヤルである。μe(g)はまた次式の様に書
ける。 Equation (9) can be understood by considering the change in chemical potential of water. The chemical equation for the reaction in which water droplets grow from water vapor is H 2 O(g)=H 2 O(l) (10). g represents gas, and l represents liquid state. Let P e be the equilibrium partial pressure of water vapor, and P be the actual water vapor pressure. If thermal equilibrium is established near the water droplet, μe(g) = μ(l) (11). Here, μe(g) is the chemical potential in the thermal equilibrium of water vapor in the gas phase, and μ(l) is the chemical potential in the water droplet. μe(g) can also be written as the following equation.
μe(g)=μo+RT lnPe (12)
実際の水蒸気の化学ポテンシヤルは分圧がPで
あるから
μ(g)=μo+RT lnP (13)
となる。分圧Pの1molの水蒸気が1molの水滴に
変化した時の自由エネルギーの変化△Gvは次式
となる。 μe(g)=μo+RT lnP e (12) Since the partial pressure of water vapor is P, the actual chemical potential of water vapor is μ(g)=μo+RT lnP (13). The change in free energy △Gv when 1 mol of water vapor with partial pressure P changes into 1 mol of water droplets is given by the following equation.
△Gv=μ(l)−μ(g)=μe(g)−μ(g)=(μo+RT lnPe
)−(μo+RT lnP)=−RT ln(P/Pe)
となり、(9)式が導出された。△Gv=μ(l)−μ(g)=μe(g)−μ(g)=(μo+RT lnP e
)−(μo+RT lnP)=−RT ln(P/P e ), and formula (9) was derived.
化学反応を伴なう場合にも同様の考え方で△
Gvを導出することができる。やはりGaAsを例に
とつて説明する。(2)の反応でGaAsを成長させる
場合を考える。原料ガス分圧をそれぞれ、P
(GaCl)、P(As4)、P(H2)、P(HCl)とし、
GaAsと平衡する分圧をそれぞれPe(GaCl)、Pe
(As4)、Pe(H2)、Pe(HCl)とする。GaAs1mol
が成長することによつてGaClは1mol、As4は1/4
mol、H2は1/2mol消費され、1molのHClが生成
される。原料ガス中の化学ポテンシヤルはそれぞ
れ
μ(GaCl)=μo(GaCl)
+RTlnP(GaCl)
μ(As4)=μo(As4)+RTlnP(As4)
μ(H2)=μo(H2)+RTlnP(H2)
μ(HCl)=μo(HCl)+RTlnP(HCl) (14)
である。GaAsと平衡している各ガスの化学ポテ
ンシヤルは
μe(GaCl)=μo(GaCl)
+RTlnPe(GaCl)
μe(As4)=μo(As4)+RTlnPe(As4)
μe(H2)=μo(H2)+RTlnPe(H2) (15)
μe(HCl)=μo(HCl)+RTlnPe(HCl)
である。GaAsと熱平衡が成立しているのである
から
μe(GaCl)+1/4μe(As4)+1/2
μe(H2)=μ(GaAs)+μe(HCl)(16)
が成立していなければならない。1molのGaAsが
析出したとき△Gvは従つて
△Gv=μ(GaAs)+μ(HCl)−μ(GaCl)−
1/4μ(As4)−1/2μ(H2)(17)
である。(17)式に(16)式を代入すれば
△Gv=−(μ(GaCl)−μe(GaCl))−1/4(μ(A
s4)−μe(As4)−1/2(μ(H2)
−μe(H2))+(μ(HCl)−μe(HCl)) (18)
となる。ガス“i”の化学反応の係数Viを考え
れば上式は
ΔGv=
〓i
Vi(μi−μie)
と書くことができる。(19)式に(15)(16)式を
代入すれば
△Gv=RT
〓i
Viln(Pi/Pie (20)
となる。水滴の成長であれば“i”はH2Oだけ
であり、VH2O=−1であるので、これを(20)式
に代入して
△Gv=−RT ln(P(H2O)/Pe(H2O)) (21)
となつて(9)式に一致する。 The same idea applies when chemical reactions are involved.
Gv can be derived. This will be explained using GaAs as an example. Consider the case where GaAs is grown by reaction (2). The raw material gas partial pressure is P
(GaCl), P(As 4 ), P(H 2 ), P(HCl),
The partial pressures in equilibrium with GaAs are P e (GaCl) and P e
(As 4 ), P e (H 2 ), and P e (HCl). GaAs1mol
By growing, GaCl becomes 1 mol and As 4 becomes 1/4
mol, H 2 is consumed 1/2 mol and 1 mol HCl is produced. The chemical potential in the source gas is μ(GaCl) = μ o (GaCl) + RTlnP (GaCl) μ (As 4 ) = μ o (As 4 ) + RTlnP (As 4 ) μ (H 2 ) = μ o (H 2 ) + RTlnP (H 2 ) μ (HCl) = μ o (HCl) + RTlnP (HCl) (14). The chemical potential of each gas in equilibrium with GaAs is μ e (GaCl) = μ o (GaCl) + RTlnP e (GaCl) μ e (As 4 ) = μ o (As 4 ) + RTlnP e (As 4 ) μ e ( H 2 ) = μ o (H 2 ) + RTlnP e (H 2 ) (15) μ e (HCl) = μ o (HCl) + RTlnP e (HCl). Since thermal equilibrium is established with GaAs, μ e (GaCl) + 1/4 μ e (As 4 ) + 1/2
μ e (H 2 ) = μ (GaAs) + μ e (HCl) (16) must hold true. When 1 mol of GaAs is precipitated, △Gv is therefore △Gv = μ(GaAs) + μ(HCl) − μ(GaCl) −
1/4μ(As 4 )−1/2μ(H 2 )(17). Substituting equation (16) into equation (17), △Gv=−(μ(GaCl) −μe (GaCl))−1/4(μ(A
s 4 ) − μ e (As 4 ) − 1/2 ( μ (H 2 ) − μ e (H 2 )) + ( μ (HCl) − μ e (HCl)) (18). Considering the coefficient Vi of the chemical reaction of gas "i", the above equation can be written as ΔGv= 〓 i Vi (μi−μi e ). Substituting equations (15) and (16) into equation (19), we get △Gv=RT 〓 i Viln(Pi/Pi e (20). In the case of water droplet growth, “i” is only H 2 O. , V H2O = -1, so by substituting this into equation (20), we get △Gv = -RT ln(P(H 2 O)/P e (H 2 O)) (21), which becomes (9 ) matches the expression.
以上の手続きにより、化学反応を伴なう場合の
△Gvが導出されたので、ハライド法であるAsCl3
法とハイドライド法であるAsH3法の△Gvの違い
について説明する。AsCl3法では原料領域におい
て温度T1における(16)式の平衡式によつて許
される量だけのGaCl、As4、H2、HClの各ガス
が存在し、それらが原料ガス成分の分圧P
(GaCl)、P(As4)、P(H2)、P(HCl)を決定す
る。成長領域において温度T2で平衡になつた後
では各分圧はPe(GaCl)、Pe(As4)、Pe(H2)、Pe
(HCl)となる。これらの値を(19)式に代入す
れば△Gvを求めることができ、標準的なGaAsの
成長条件であるT1=850℃、T2=750℃AsCl3の
濃度=3×10-3atmにおいて△Gvを求めれば−
2〜−3kcal/molと有限の値となる。この値は、
上記成長条件で反応管内壁への結晶の析出がほと
んどないことから3次元核形成のできない、負で
はあるが充分に絶対値の小さな△Gvの値である
と考えてよい。 Through the above procedure, △Gv in the case involving a chemical reaction was derived, so AsCl 3 which is the halide method
We will explain the difference in △Gv between the AsH3 method and the hydride method. In the AsCl 3 method, each gas of GaCl, As 4 , H 2 , and HCl exists in the raw material region in the amount allowed by the equilibrium equation (16) at temperature T 1 , and these gases increase the partial pressure of the raw material gas components. P
(GaCl), P(As 4 ), P(H 2 ), and P(HCl) are determined. After reaching equilibrium at temperature T 2 in the growth region, the partial pressures are P e (GaCl), P e (As 4 ), P e (H 2 ), P e
(HCl). By substituting these values into equation (19), △Gv can be found, and the standard GaAs growth conditions are T 1 = 850℃, T 2 = 750℃, AsCl 3 concentration = 3×10 -3 If we find △Gv at atm, −
It has a finite value of 2 to -3 kcal/mol. This value is
Since there is almost no precipitation of crystals on the inner wall of the reaction tube under the above growth conditions, it can be considered that the value of ΔGv is negative but has a sufficiently small absolute value that does not allow three-dimensional nucleation.
ところがAsH3法においてはハイドライド法の
説明で詳しく述べた様に原料ガス中にほとんど
HClガスが存在しない。従つて(19)式で定義さ
れる△Gvの中でHClに関係する項ln(P(HCl)/
Pe(HCl))が−∞となり、その化学反応の係数
VHCl=1であることから、結局△Gv=−∞とな
る。これを3次元核形成理論の立場から見れば、
ハイドライド法においては3次元核を作ろうとす
る熱力学的な“driving force”が極めて大きく、
必ず3次元核を形成することを意味する。 However, in the AsH 3 method, as explained in detail in the explanation of the hydride method, almost no
No HCl gas present. Therefore, in △Gv defined by equation (19), the term ln(P(HCl)/
P e (HCl)) becomes −∞, and the coefficient of the chemical reaction is
Since V HCl = 1, △Gv = -∞. If we look at this from the standpoint of three-dimensional nucleation theory,
In the hydride method, the thermodynamic "driving force" that tries to create a three-dimensional nucleus is extremely large.
This means that a three-dimensional nucleus is always formed.
△Gvに対するハライド法とハイドライド法の
以上の説明から明らかな様に3次元核を反応管内
壁に形成させないようにするためには、本発明の
様に原料ガス中に金属原料に接触させないでHCl
ガスを加えてやれば△Gvを負ではあるが絶対値
の小さな値とすることができ、3次元核形成を抑
制することができる。 As is clear from the above explanation of the halide method and hydride method for △Gv, in order to prevent the formation of three-dimensional nuclei on the inner wall of the reaction tube, it is necessary to add HCl to the raw material gas without bringing it into contact with the metal raw material, as in the present invention.
By adding gas, ΔGv can be set to a negative but small absolute value, and three-dimensional nucleation can be suppressed.
反応管内壁への3次元核の形成を抑制する目的
のためには△Gvを負ではあるが、絶対値の小さ
な値とすれば良いのであるから、混合すべきガス
の種類はHClだけに限らない。混合した後で、
族元素を輸送するために用いたハロゲンの水素化
物が発生するものであれば何であつてもかまわな
い。HClガスの代りにHBrガスを加えれば以下の
入れ替え反応
GaCl+HBr=GaBr+HCl (22)
が起こつて、原料ガス中にHClおよびGaBrガス
が存在する様になる。すなわちGa元素はCl化物
として輸送され、2つの成長反応
GaCl+1/4As4+1/2H2=GaAs+HCl
GaBr+1/4As4+1/2H2=GaAs+HBr
(23)
が同時に起こつてGaAsを成長させる。このよう
に複数の成長反応によつて固相が析出する場合に
は(19)式を拡張しなければならない。 For the purpose of suppressing the formation of three-dimensional nuclei on the inner wall of the reaction tube, it is sufficient to set △Gv to a negative but small absolute value, so the type of gas to be mixed is limited to HCl only. do not have. After mixing,
Any material may be used as long as it generates a hydride of the halogen used to transport the group element. If HBr gas is added instead of HCl gas, the following exchange reaction GaCl + HBr = GaBr + HCl (22) occurs, and HCl and GaBr gases become present in the source gas. In other words, Ga element is transported as a chloride, and two growth reactions GaCl + 1/4As 4 + 1/2H 2 = GaAs + HCl GaBr + 1/4As 4 + 1/2H 2 = GaAs + HBr
(23) occur simultaneously to grow GaAs. In this way, when a solid phase is precipitated by multiple growth reactions, equation (19) must be expanded.
以下で、複数の成長反応が同時に起こる場合の
△Gvの導出について説明する。結晶の析出反応
がM個存在し、j番目の析出反応の化学反応式の
係数Vij(j=1、…M)とすれば、j番目の化学
反応で1molの結晶が析出した場合の自由エネル
ギー変化△Gvjは
△Gvj=RT
〓i
Vijln(Pi/Pie) (24)
(j=1…M)
となる。従つて、複数の化学反応によつてそれぞ
れXj(j=1…M)のモル分率で同時に結晶を析
出した場合には
△Gv=
〓i
Xj△Gvj (25)
となる。(24)式を(25)式に代入すれば
△Gv=
〓i
Xj(RT
〓i
Vij)ln(Pi/Pie)
=RT
〓i
(
〓i
XjVij)ln(Pi/Pie) (26)
となる。 Below, we will explain how to derive ΔGv when multiple growth reactions occur simultaneously. If there are M crystal precipitation reactions, and the coefficient Vij of the chemical reaction equation for the j-th precipitation reaction is Vij (j=1,...M), then the free energy when 1 mol of crystals is precipitated in the j-th chemical reaction is The change △Gvj is △Gvj=RT 〓 i Vijln(Pi/Pi e ) (24) (j=1...M). Therefore, when crystals are precipitated simultaneously at a mole fraction of Xj (j=1...M) through multiple chemical reactions, △Gv= 〓 i Xj△Gvj (25). Substituting equation (24) into equation (25), △Gv= 〓 i Xj (RT 〓 i Vij ) ln (Pi/Pi e ) = RT 〓 i ( 〓 i ) becomes.
HClの代りにHBrを加えた場合には(26)式に
よつて△Gvを計算することができる。このとき
には原料ガス中に(23)の析出反応の生成ガスで
あるHClとHBrが存在するため△Gvは−∞では
なく、負の有限な量になり、HBrの量を多くす
ることによつて、△Gvは負ではあるがその絶対
値のより小さな値となり、反応管内壁への3次元
核形成が抑制される。 When HBr is added instead of HCl, ΔGv can be calculated using equation (26). At this time, since HCl and HBr, which are the gases produced by the precipitation reaction (23), are present in the raw material gas, △Gv is not -∞ but a negative finite amount, and by increasing the amount of HBr, , ΔGv is negative, but its absolute value is smaller, and three-dimensional nucleation on the inner wall of the reaction tube is suppressed.
HClの代りにHIを導入しても上の説明と類似
の議論によつて△Gvを負ではあるが絶対値の小
さな値とすることができ反応管内壁への3次元核
形成を抑制することができる。 Even if HI is introduced instead of HCl, △Gv can be made negative but small in absolute value by a similar argument to the above explanation, and three-dimensional nucleation on the inner wall of the reaction tube can be suppressed. Can be done.
HClの代りにAsCl3を導入しても同じ効果が得
られる。このときAsCl3は混合された後キヤリヤ
ーガスH2と(1)式に従つて分解反応を起こして
HClを生成し、(19)式で求められる△Gvは加え
るAsCl3の量が多い程負で絶対値の小さな値とな
り、反応管内壁への3次元核形成が抑制される。 The same effect can be obtained by introducing AsCl 3 instead of HCl. At this time, AsCl 3 is mixed with carrier gas H 2 and undergoes a decomposition reaction according to equation (1).
The larger the amount of AsCl 3 added, the smaller the absolute value of ΔGv obtained by generating HCl, and the smaller the absolute value, which suppresses three-dimensional nucleation on the inner wall of the reaction tube.
HClの代りにAsBr3を導入しても同じ効果が得
られる。このときAsBr3は混合された後キヤリヤ
ーガスのH2と次式
AsBr3+3/2H2=1/4As4+3HBr (27)
によつて分解反応を起こし、生成したHBrガス
は更に(22)式に従つて入れ替え反応を起こし、
(26)式で求められる△Gvは負ではあるが、絶対
値の小さな値となつて反応管内壁への3次元核形
成を抑制する。 The same effect can be obtained by introducing AsBr 3 instead of HCl. At this time, after AsBr 3 is mixed, a decomposition reaction occurs with H 2 of the carrier gas according to the following equation AsBr 3 + 3/2H 2 = 1/4 As 4 + 3HBr (27), and the generated HBr gas is further expressed in equation (22). Therefore, an exchange reaction occurs,
Although ΔGv determined by equation (26) is negative, it has a small absolute value and suppresses three-dimensional nucleation on the inner wall of the reaction tube.
HClの代りにCl2を導入しても同じ効果が得ら
れる。このときCl2は混合された後キヤリヤーガ
スのH2と次式
Cl2+H2=2HCl (28)
によつてHClガスを生成し、(19)式で求められ
る△Gvは負ではあるが絶対値の充分に小さな値
となつて反応管内壁への3次元核形成を抑制す
る。 The same effect can be obtained by introducing Cl 2 instead of HCl. At this time, after Cl 2 is mixed with H 2 of the carrier gas, HCl gas is generated by the following equation: Cl 2 + H 2 = 2HCl (28), and △Gv obtained from equation (19) is a negative, but absolute value. has a sufficiently small value to suppress three-dimensional nucleation on the inner wall of the reaction tube.
HClの代りにBr2を導入しても同じ効果が得ら
れる。このとき、Br2は混合された後キヤリヤー
ガスのH2と次式
Br2+H2=2HBr (29)
によつてHBrガスを生成し、(22)式の入れ替え
反応が起こり(26)式で求められる△Gvは負で
はあるが、絶対値の充分に小さな値となつて反応
管内壁への3次元核形成を抑制する。 The same effect can be obtained by introducing Br 2 instead of HCl. At this time, after Br 2 is mixed with H 2 of the carrier gas, HBr gas is generated by the following equation Br 2 + H 2 = 2HBr (29), and the exchange reaction of equation (22) occurs, which is calculated by equation (26). Although the resulting ΔGv is negative, its absolute value is sufficiently small to suppress three-dimensional nucleation on the inner wall of the reaction tube.
以上の説明では−化合物半導体のひとつと
してGaAsを取上げて、HCl、HBr、HI、AsCl3、
AsBr3、Cl2、Br2を原料金属(Ga)をバイパス
する管より加えることの効果を説明したが、この
効果はGaAsに限られる訳ではなく族元素とし
て、B、Al、Ga、In、のひとつ以上と族元素
のN、P、As、Sbのひとつ以上から成る、二元、
あるいは三元、四元、をはじめとする多元−
化合物混晶半導体のハイドライド法によるハライ
ド気相成長法に有効なことは、明らかである。 In the above explanation, GaAs is taken up as one of the compound semiconductors, and HCl, HBr, HI, AsCl 3 ,
We have explained the effect of adding AsBr 3 , Cl 2 , and Br 2 through a tube that bypasses the raw metal (Ga), but this effect is not limited to GaAs, but also applies to B, Al, Ga, In, and one or more of the group elements N, P, As, Sb,
Or multiple elements including ternary, quaternary, etc.
It is clear that this method is effective for halide vapor phase epitaxy using the hydride method for compound mixed crystal semiconductors.
以上本発明の原理について述べたが、以下に実
施例をもつて説明する。 The principle of the present invention has been described above, and will be explained below using examples.
本発明を実施するに要する製造装置は、その基
本的構成において前記従来技術の説明に用いた第
2図のハイドライド法によるハロゲン気相成長層
置をそのまま使用できる。3元系以上の化合物混
晶半導体を成長させる場合については族金属原
料を納める部分を互いに独立した部分で構成した
装置を用いればよい。 The basic structure of the manufacturing apparatus required to carry out the present invention can use the halogen vapor phase epitaxy layer deposition by the hydride method shown in FIG. 2 used in the explanation of the prior art as is. When growing a ternary or higher compound mixed crystal semiconductor, it is sufficient to use an apparatus in which the parts containing the group metal raw materials are made up of mutually independent parts.
以下の実施例に使用した装置の概要は、反応管
が外径50mmの高純度石英管で、族金属原料を納
める位置と成長基板を納める位置との間隔が30
cm、バイパス管の出口と成長基板との間隔が20cm
である。 The outline of the apparatus used in the following examples is that the reaction tube is a high-purity quartz tube with an outer diameter of 50 mm, and the distance between the position where the group metal raw material is stored and the position where the growth substrate is stored is 30 mm.
cm, the distance between the outlet of the bypass tube and the growth substrate is 20 cm
It is.
実施例 1
GaAsのハイドライド法によるハロゲン気相成
長
族金属原料として99.99999%のGa約50gを高
純度石英製ボードに納め、800℃に保つ、そこに
1%のHClガスを含む水素流を毎分500c.c.で流す。
バイパス管からは0.5%のAsH3ガスと0.15%の
HClガスを含む水素流を毎分1000c.c.で流す。成長
基板には{100}から<110>方向に2゜傾けた
GaAs単結晶ウエハーを用い、750℃で反応させ
る。この条件で30分間維持することにより約9μ
mの厚さを有するGaAsの鏡面エピタキシヤル成
長層を得た。目視観察によれば、バイパス管の出
口から基板結晶までの間の反応管内壁への3次元
核形成による結晶の析出はなかつた。成長速度の
時間依存性を調べるために、10分間毎にバイパス
管からH2Sガスを200ppmの濃度で30秒間反応管
内に導入してドーピングを行ない、60分間成長を
行なつた。成長したGaAsの基板結晶を壁開し、
壁開面をHF+H2O2+H2Oのエツチング液でエツ
チングすると不純物濃度の違いによつてGaAsの
エツチング速度が異なり10分毎のドーピングした
GaAs層が層状に見られる。これらの層と層との
距離を測定して10分毎の平均の成長速度を求める
ことができる。第4図には、このようにして求め
たGaAsの成長速度を、0.15%のHClをバイパス
管から導入しないとき(A)と導入したとき(B)につい
てグラフにした。HClガスを導入しないとき、目
視観察によれば明らかにGaAsの結晶が反応管内
壁に析出しており、成長速度の減少はこの3次元
核成長が原因するものと考えられる。HClガスを
導入した時間には3次元核が形成されず成長速度
は一定値0.15μm/minを保つており、本発明の
効果は明らかである。Example 1 Halogen vapor phase growth of GaAs by hydride method Approximately 50 g of 99.99999% Ga as a group metal raw material is placed in a high-purity quartz board and kept at 800°C, where a hydrogen flow containing 1% HCl gas is applied every minute. Flow at 500c.c.
From the bypass pipe 0.5% AsH3 gas and 0.15%
Flow a hydrogen stream containing HCl gas at 1000 c.c. per minute. The growth substrate was tilted 2° from {100} to <110> direction.
A GaAs single crystal wafer is used and the reaction is carried out at 750℃. By maintaining this condition for 30 minutes, approximately 9μ
A mirror epitaxial growth layer of GaAs with a thickness of m was obtained. According to visual observation, no crystals were deposited due to three-dimensional nucleation on the inner wall of the reaction tube between the outlet of the bypass tube and the substrate crystal. In order to investigate the time dependence of the growth rate, doping was performed by introducing H 2 S gas into the reaction tube from the bypass tube at a concentration of 200 ppm for 30 seconds every 10 minutes, and growth was performed for 60 minutes. The grown GaAs substrate crystal is wall-opened,
When the wall opening was etched with an etching solution of HF + H 2 O 2 + H 2 O, the etching rate of GaAs varied depending on the impurity concentration, and doping was performed every 10 minutes.
The GaAs layer can be seen in layers. By measuring the distance between these layers, the average growth rate per 10 minutes can be determined. In FIG. 4, the growth rate of GaAs determined in this manner is plotted as a graph when 0.15% HCl is not introduced from the bypass tube (A) and when it is introduced (B). When no HCl gas was introduced, visual observation showed that GaAs crystals were clearly precipitated on the inner wall of the reaction tube, and the decrease in growth rate was thought to be caused by this three-dimensional nuclear growth. During the time that HCl gas was introduced, no three-dimensional nuclei were formed and the growth rate remained constant at 0.15 μm/min, which clearly demonstrates the effectiveness of the present invention.
実施例 2
InPのハイドライド法によるハロゲン気相成長
法
族金属原料として99.9999%のIn約50gを高
純度石英製ボートに納め、800℃に保つ、そこに
1%のHClガスを含む水素流を毎分500c.c.で流す。
バイパス管からは0.5%のAsH3ガスと0.015%の
HClガスを含んだ水素流を毎分1000c.c.で流す。成
長基板は{100}面から<110>方向に2゜傾いた面
を持つInP単結晶を用いた。700℃の成長温度で
30分間維持することによつて約3.6μmの厚さを有
するInPの鏡面エピタキシヤル成長層を得た。目
視観察によればバイパス管の出口から基板結晶ま
での間の反応管内壁への3次元核形による結晶の
析出はなかつた。この条件で10回のInPの成長を
試みたところ成長膜厚は、その80%が±5%以内
に入つており、成長速度の再現性が非常に良いこ
とが確認された。HClガスをバイパス管から導入
しない場合には成長速度の再現性が悪く、最大7
〜8倍の成長速度のばらつきが見られ、本発明の
効果は明らかであつた。Example 2 Halogen vapor phase growth method using the hydride method for InP Approximately 50 g of 99.9999% In as a group metal raw material was placed in a high-purity quartz boat, kept at 800°C, and a hydrogen stream containing 1% HCl gas was added every time. Run at 500 c.c. per minute.
From the bypass pipe 0.5% AsH3 gas and 0.015%
Flow a hydrogen stream containing HCl gas at 1000 c.c. per minute. The growth substrate used was an InP single crystal with a plane tilted 2° from the {100} plane toward the <110> direction. At a growth temperature of 700℃
By maintaining this for 30 minutes, a specular epitaxial growth layer of InP having a thickness of about 3.6 μm was obtained. According to visual observation, there was no precipitation of crystals due to three-dimensional nuclear shapes on the inner wall of the reaction tube between the outlet of the bypass tube and the substrate crystal. When InP was grown 10 times under these conditions, 80% of the grown film thicknesses were within ±5%, confirming that the reproducibility of the growth rate was very good. If HCl gas is not introduced from the bypass pipe, the reproducibility of the growth rate is poor, and the maximum
A variation in growth rate of ~8 times was observed, and the effect of the present invention was clear.
実施例 3
InGaAsP混晶のハイドライド法によるハロゲ
ン気相成長法
第5図の様に族金属原料としてGa6とIn11を
それぞれ40g高純度石英製ボートに入れ、独立し
た構成の部屋に納め、800℃に保つた。第1の
HClガス導入管12から0.14%のHClガスを含ん
た水素流を毎分250c.c.で導入し、原料金属Gaと反
応させた。第2のHClガス導入管13から2.4%
のHClガスを含んだ水素流を毎分250c.c.で導入し、
原料金属Inと反応させた。バイパス管9からは
0.18%のAsH3ガスと0.4%のPH3ガスと0.09%の
HClガスを含む水素流を毎分1000c.c.で導入し680
℃でInPの(100)基板結晶14上にInGaAsP混
晶半導体を成長させた。10分間上記条件を維持さ
せたところ、約3μm厚さのInGaAsPの鏡面エピ
タキシヤル成長層を得た。X線ロツキングカーブ
によつてこの成長層の格子定数を調べた。HClガ
スをバイパス管より導入したときには第6図Bの
様に鋭いInPの回折ピークとInGaAsPの回折ピー
クが見え、InGaAsPの格子定数が成長方向に一
定値となり、混晶の組成が均一であることを証拠
だてている。しかしHClガスをバイパス管から導
入しない場合にはロツキングカーブは第6図Aの
様に多くのピークを持つものとなり反応管内壁へ
の3次元核形成による結晶の析出のために成長し
たInGaAsPは成長方向に組成が変化したことを
証拠だてている。このように、本発明が混晶半導
体を気相成長させる場合にその組成を均一なもの
にする上で有効なことが明らかである。Example 3 Halogen vapor phase growth method using the hydride method for InGaAsP mixed crystal As shown in Figure 5, 40g each of Ga6 and In11 as group metal raw materials were placed in a high purity quartz boat, placed in an independent room, and heated to 800℃. I kept it. first
A hydrogen flow containing 0.14% HCl gas was introduced from the HCl gas inlet pipe 12 at a rate of 250 c.c. per minute to react with the raw metal Ga. 2.4% from the second HCl gas introduction pipe 13
A flow of hydrogen containing HCl gas was introduced at a rate of 250 c.c. per minute,
It was reacted with the raw metal In. From bypass pipe 9
0.18% AsH3 gas and 0.4% PH3 gas and 0.09%
Introducing a hydrogen flow containing HCl gas at a rate of 1000c.c.680
An InGaAsP mixed crystal semiconductor was grown on an InP (100) substrate crystal 14 at ℃. When the above conditions were maintained for 10 minutes, a specular epitaxial growth layer of InGaAsP with a thickness of about 3 μm was obtained. The lattice constant of this grown layer was investigated using an X-ray rocking curve. When HCl gas is introduced through the bypass pipe, sharp diffraction peaks of InP and InGaAsP can be seen as shown in Figure 6B, indicating that the lattice constant of InGaAsP is constant in the growth direction and the composition of the mixed crystal is uniform. proves that. However, if HCl gas is not introduced from the bypass tube, the rocking curve will have many peaks as shown in Figure 6A, and the InGaAsP that has grown due to the precipitation of crystals due to three-dimensional nucleation on the inner wall of the reaction tube. This provides evidence that the composition changed in the direction of growth. Thus, it is clear that the present invention is effective in making the composition uniform when a mixed crystal semiconductor is grown in a vapor phase.
第1図は、ハライド法による従来のハロゲン気
相成長装置を説明するための図である。第2図は
ハイドライド法による従来のハロゲン気相成長装
置を説明するための図である。第3図は3次元核
形成の自由エネルギー△Gを核の大きさγの関数
としてグラフにしたもので、△Gvをパラメータ
として描いてある。△Gvが負ではあるが、絶対
値の小さな値であれば臨界核の大きさγ*が大き
くなりその時の自由エネルギー△G*も大きくな
つて3次元核の形成が抑制される様子を説明する
ものである。第4図は本発明をGaAsのハイドラ
イド法によるハロゲン気相成長に適用したときの
効果を示す図で、AはHClを導入しないときBは
HClを導入したときの時間による成長速度の変化
の様子を図示している。第5図は本発明を
InGaAsPのハイドライド法によるハロゲン気相
成長に適用する場合の装置を説明するための図で
ある。第6図はInGaAsPのハイドライド法によ
るハロゲン気相成長に適用したときの効果を説明
するための図でHClを導入しない場合のX線ロツ
キングカーブA図とHClを導入したときのX線ロ
ツキングカーブB図である。
図において、1……AsCl3を含む水素の導入
管、2……原料GaAs、3……成長領域、4……
基板GaAs結晶、5,10……バイパス管の出口
と基板結晶の間の反応管内壁、6……原料金属
Ga、7,12,13……HClを含む水素流の導
入管、8……混合領域、9……バイパス管、11
……原料金属In、14……基板InP結晶を示す。
FIG. 1 is a diagram for explaining a conventional halogen vapor phase growth apparatus using the halide method. FIG. 2 is a diagram for explaining a conventional halogen vapor phase growth apparatus using the hydride method. FIG. 3 is a graph of the free energy of three-dimensional nucleation ΔG as a function of the nucleus size γ, with ΔGv as a parameter. Although △Gv is negative, if the absolute value is small, the size of the critical nucleus γ * will increase, the free energy △G * will also increase, and the formation of three-dimensional nuclei will be suppressed. It is something. Figure 4 shows the effect when the present invention is applied to halogen vapor phase epitaxy of GaAs by the hydride method, where A is when no HCl is introduced and B is
The diagram shows how the growth rate changes over time when HCl is introduced. Figure 5 shows the present invention.
FIG. 2 is a diagram for explaining an apparatus applied to halogen vapor phase growth of InGaAsP by a hydride method. Figure 6 is a diagram to explain the effect when applied to halogen vapor phase growth using the hydride method for InGaAsP, showing the X-ray rocking curve A diagram when HCl is not introduced and the X-ray rocking curve when HCl is introduced. It is a curve B diagram. In the figure, 1... hydrogen introduction tube containing AsCl 3 , 2... raw material GaAs, 3... growth region, 4...
Substrate GaAs crystal, 5, 10... Inner wall of reaction tube between outlet of bypass tube and substrate crystal, 6... Raw metal
Ga, 7, 12, 13...Introduction pipe for hydrogen flow containing HCl, 8...Mixing region, 9...Bypass pipe, 11
. . . Raw metal In, 14 . . . Indicates substrate InP crystal.
Claims (1)
ゲン気相成長方法において、族原料とキヤリア
ーガスで希釈されたハロゲン化水素ガスを反応さ
せて族元素のハロゲン化物を生成し、族原料
より下流でかつ族元素ハイドライドガスが成長
装置内に注入される位置と同じかまたは上流に、
ハロゲンガス、ハロゲン化水素あるいは族元素
ハライドを導入することを特徴とする−族化
合物半導体のハイドライド法ハロゲン気相成長
法。1 In the hydride method halogen vapor phase growth method for group compound semiconductors, a group raw material and a hydrogen halide gas diluted with a carrier gas are reacted to produce a group element halide, and a group element hydride is produced downstream of the group raw material. At the same location or upstream from where the gas is injected into the growth apparatus,
A hydride halogen vapor phase growth method for a - group compound semiconductor, which is characterized by introducing a halogen gas, a hydrogen halide, or a group element halide.