JPH0362820A - Curing resin composition - Google Patents

Curing resin composition

Info

Publication number
JPH0362820A
JPH0362820A JP19915289A JP19915289A JPH0362820A JP H0362820 A JPH0362820 A JP H0362820A JP 19915289 A JP19915289 A JP 19915289A JP 19915289 A JP19915289 A JP 19915289A JP H0362820 A JPH0362820 A JP H0362820A
Authority
JP
Japan
Prior art keywords
epoxy resin
curing
resin composition
curable resin
compound
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
JP19915289A
Other languages
Japanese (ja)
Inventor
Yuji Kunitake
国武 憂璽
Junji Nanbu
南部 順治
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
DIC Corp
Original Assignee
Dainippon Ink and Chemicals Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dainippon Ink and Chemicals Co Ltd filed Critical Dainippon Ink and Chemicals Co Ltd
Priority to JP19915289A priority Critical patent/JPH0362820A/en
Publication of JPH0362820A publication Critical patent/JPH0362820A/en
Ceased legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
(57) [Summary] This bulletin contains application data before electronic filing, so abstract data is not recorded.

Description

【発明の詳細な説明】 〔産業上の利用分野〕 本発明は改良された硬化性樹脂組成物に関する。[Detailed description of the invention] [Industrial application field] This invention relates to improved curable resin compositions.

さらに詳細には、本発明は4,4′−ジヒドロキシジフ
ェニルスルホン(以下、ビスフェノールSと略称する。
More specifically, the present invention relates to 4,4'-dihydroxydiphenyl sulfone (hereinafter abbreviated as bisphenol S).

)に基ずく、式 なる構造の繰り返し単位を有する特定のエポキシ樹脂と
アミン系エポキシ樹脂硬化剤とを必須の皮膜形成性成分
として含んで威る、とりわけ、硬化触媒ないしは硬化促
進剤の使用量を低減することができ、しかも、硬化物の
可撓性および耐湿性が改善された、粉体塗料あるいは絶
縁塗料などとして有用なる硬化性樹脂組成物に関する。
), which contains a specific epoxy resin having a repeating unit with the structure of the formula and an amine-based epoxy resin curing agent as essential film-forming components, and in particular, the amount of curing catalyst or curing accelerator to be used. The present invention relates to a curable resin composition useful as a powder coating, an insulating coating, etc., which can reduce the amount of moisture and has improved flexibility and moisture resistance of the cured product.

〔従来の技術〕[Conventional technology]

一般に、エポキシ樹脂なるものは、電気特性、機械特性
ならびに耐食性などにずくれる処から、電気製品や塗料
などの各分野で幅広く利用されてはいる。
In general, epoxy resins are widely used in various fields such as electrical products and paints because of their excellent electrical properties, mechanical properties, and corrosion resistance.

ところで、かかるエポキシ樹脂は、通常、アミノ系硬化
剤により硬化させて用いられるが、−層すくれた硬化物
を得るためには、加熱によって、反応率を上げるのが一
般的な方法であり、各種のエポキシ塗料やエポキシ絶縁
材料などは、実際、加熱硬化の方法により用いられてい
る。
By the way, such epoxy resins are usually used after being cured with an amino curing agent, but in order to obtain a cured product with thin layers, it is a common method to increase the reaction rate by heating. Various epoxy paints and epoxy insulating materials are actually used by heat curing methods.

しかしながら、こうした加熱硬化方式にしても、その加
熱温度が150°C以上という高温になる場合には、ど
うしても、素材に与える温度の影響や、エネルギー消費
などの面で問題層も多い。
However, even with such a heat curing method, there are many problems in terms of the effect of temperature on the material and energy consumption when the heating temperature is as high as 150° C. or higher.

したがって、硬化温度の低減化に対する要求も強くなっ
ている。
Therefore, there is an increasing demand for lower curing temperatures.

そこで、目下の処、かかる温度低減法として採用されて
いるのが、使用する硬化触媒ないしは硬化促進剤の量を
増大させるという専らの手段である。
Therefore, the method currently employed for reducing the temperature is to increase the amount of curing catalyst or curing accelerator used.

すなわち、活性水素をもったアミンによる硬化方式にあ
っては、硬化触媒(硬化促進剤)として、3級アくン化
合物、アルコール性化合物、フェノール性化合物または
有機酸化合物などが添加使用されているが、そのさい、
かかる触媒化合物の添加使用量を増大せしめることによ
って、硬化温度の低減化が図られている。
That is, in a curing method using an amine having active hydrogen, a tertiary amine compound, an alcoholic compound, a phenolic compound, or an organic acid compound is added as a curing catalyst (curing accelerator). However, at that time,
By increasing the amount of such catalyst compound added, the curing temperature is reduced.

また、3級アミノ基または4級アンモニウム塩基を有す
る化合物を用いて、エポキシ樹脂のアニオン重合方式に
よる硬化を行なう場合にあっても、かかるアニオン重合
触媒化合物の使用量を増大せしめることによって、硬化
温度の低減化が図られている。
Furthermore, even when curing an epoxy resin by an anionic polymerization method using a compound having a tertiary amino group or a quaternary ammonium base, the curing temperature can be adjusted by increasing the amount of such anionic polymerization catalyst compound. Efforts are being made to reduce this.

ところが、こうした在来の方法に従う場合には、どうし
ても、添加される低分子量極性物質の使用量が増える処
から、硬化物の耐水性などの上で悪影響が認められるよ
うになる。
However, when such conventional methods are followed, the amount of low-molecular-weight polar substances added inevitably increases, which causes an adverse effect on the water resistance of the cured product.

しかも、上述したような活性水素をもったアミンによる
硬化方式による場合において、就中、3級アミノ基また
は4級アンモニウム塩基を有する化合物を用いるさいに
は、こうした3級アミノ基含有化合物または4級アンモ
ニウム塩基含有化合物が、そもそも、エポキシ樹脂のア
ニオン重合機能を有するものである処から、これらの硬
化触媒(硬化促進剤)が多量に用いられると、活性水素
とエポキシ樹脂との反応以外に、エポキシ樹脂同志のア
ニオン重合が無視し得なくなり、得られる硬化物が可撓
性の劣る、脆いものになってしまうという欠点があった
。
Moreover, in the case of the curing method using an amine having active hydrogen as described above, especially when using a compound having a tertiary amino group or a quaternary ammonium base, such a compound containing a tertiary amino group or a quaternary ammonium base is Since ammonium base-containing compounds originally have the function of anionic polymerization of epoxy resin, when these curing catalysts (curing accelerators) are used in large quantities, in addition to the reaction between active hydrogen and epoxy resin, epoxy resin The disadvantage is that anionic polymerization between resins cannot be ignored, resulting in a cured product with poor flexibility and brittleness.

〔発明が解決しようとする課題〕[Problem to be solved by the invention]

このように、エポキシ樹脂におけるアミン硬化システム
については、その加熱硬化温度の低減化が求められてい
るけれども、従来の技術に従う限り、得られる硬化物の
耐水性や可撓性などが損われてしまうという、未解決の
課題の存在に特に注目すべきであろう。
As described above, there is a need to reduce the heat curing temperature of amine curing systems for epoxy resins, but as long as conventional techniques are followed, the water resistance and flexibility of the resulting cured products will be impaired. Particular attention should be paid to the existence of unresolved issues.

そこで、本発明者らは、こうした現状の認識と、従来技
術における種々の未解決課題の抜本的な解決との上に立
って、この種のエポキシ樹脂−アミノ系硬化剤なる硬化
性樹脂組成物の、真の意味での実用化を図るべく、鋭意
、研究に着手した。
Therefore, based on the recognition of the current situation and the fundamental solution to various unresolved problems in the prior art, the present inventors have developed a curable resin composition of this type as an epoxy resin-amino curing agent. In order to put this into practical use in the true sense of the word, we began earnest research.

したがって、本発明が解決しようとする課題は、−にか
かって、硬化物の耐水性および可撓性などを損うことな
く、極力、加熱硬化温度を低減化せしめることができる
。極めて有用なるエポキシ樹脂を、そして、該樹脂を必
須成分の一つとして含んで成る、極めて有用なる硬化性
樹脂組成物を提供することである。
Therefore, the problem to be solved by the present invention is to reduce the heat curing temperature as much as possible without impairing the water resistance and flexibility of the cured product. An object of the present invention is to provide an extremely useful epoxy resin and an extremely useful curable resin composition comprising the resin as one of its essential components.

〔課題を解決するための手段〕[Means to solve the problem]

本発明者らは上述した如き解決すべき課題の抜本的な解
決に照準を合わせて鋭意検討を重ねた結果、ビスフェノ
ールSという特別の化合物を原料成分の一つとして用い
て、式 で示されるような構造単位をエポキシ樹脂に導入せしめ
ることにより、上述した如き従来技術における未解決課
題の悉くか解決されることを見い出すに及んで、本発明
を完成させるに到った。
The inventors of the present invention have conducted extensive studies with the aim of fundamentally solving the problems to be solved as described above, and as a result, using a special compound called bisphenol S as one of the raw material components, as shown in the formula: The present invention has been completed by discovering that all of the unresolved problems in the prior art as described above can be solved by introducing a structural unit into an epoxy resin.

すなわち、本発明は必須の成分として、式なる繰り返し
単位を主構成単位として有する、ビスフェノールSを必
須の原料成分として用いて得られるエポキシ樹脂(A、
 )と、アミン系エポキシ樹脂硬化剤(B)とを含んで
成る、とりわけ、加熱硬化温度の低減化が可能であって
、しかも、改善された耐水性および可撓性などを有する
、極めて有用なる硬化性樹脂組成物を提供しようとする
ものである。
That is, the present invention is an epoxy resin (A,
) and an amine-based epoxy resin curing agent (B), which is particularly useful and which can reduce the heating curing temperature and has improved water resistance and flexibility. The present invention aims to provide a curable resin composition.

ここにおいて、上記したエポキシ樹脂(A)とは、分子
内に1個を超えるエポキシ基を持った化合物であって、
しかも、主要構造単位として、前掲の式CI)で示され
る繰り返し単位を含んでいるものを指称する。
Here, the above-mentioned epoxy resin (A) is a compound having more than one epoxy group in the molecule,
Moreover, it refers to a compound containing a repeating unit represented by the above-mentioned formula CI) as a main structural unit.

つまり、特徴的な構成単位としてビスフェノールSに由
来する、前掲の式(r)で示される繰り返し単位が導入
されたエポキシ樹脂を指称するものと理解されたい。
In other words, it should be understood that it refers to an epoxy resin into which a repeating unit derived from bisphenol S and represented by the above-mentioned formula (r) is introduced as a characteristic structural unit.

当該エポキシ樹脂(A)を調製するに当って、このビス
フェノールS以外の原料成分としては、特に限が無いが
、そのうちでも特に代表的なもののみを例示するに止め
れば、ビスフェノールAエピクロルヒドリン縮合物また
は該縮合物形成性M分、ビスフェノールF−エピクロル
ヒドリン縮合物または該縮合物形成性成分、あるいは、
フェノール類のアルキレンオキサイド付加アルコールと
エピクロルヒドリンとの縮合反応生成物またはこれらの
縮合物形成性各成分などであり、それらは単独でも、2
種以上の併用でもよいことは、勿論である。
In preparing the epoxy resin (A), there are no particular limitations on the raw material components other than bisphenol S, but only the most representative ones are listed, such as bisphenol A epichlorohydrin condensate or The condensate-forming M component, the bisphenol F-epichlorohydrin condensate or the condensate-forming component, or
It is a condensation reaction product of an alkylene oxide addition alcohol of phenols and epichlorohydrin, or each of these condensate-forming components.
Of course, more than one species may be used in combination.

当該エポキシ樹脂(A)中に導入すべきビスフェノール
Sの量、つまり、導入率としては、好ましくは、3〜6
0重量%、より好ましくは、5〜30重量%なる範囲内
が適切である。
The amount of bisphenol S to be introduced into the epoxy resin (A), that is, the introduction rate is preferably 3 to 6.
A suitable range is 0% by weight, more preferably 5 to 30% by weight.

3重量%未満の場合には、どうしても、充分な硬化温度
の低減化が果され難くなるし、一方、60重量%を超え
る場合には、却って、耐水性を損うこととなり易いので
、いずれの場合も好ましくない。
If it is less than 3% by weight, it will be difficult to achieve a sufficient reduction in curing temperature, while if it exceeds 60% by weight, water resistance will be likely to be impaired. The case is also unfavorable.

本発明において用いられる硬化剤システムとして、特に
代表的なもののみを例示すめに止めれば、第一に、前掲
された如きエポキシ樹脂(A)中のエポキシ基と反応し
うる活性水素を持った1級および/または2級アミノ基
を含有する化合物をそのまま用い、あるいは、これらの
アミノ基含有化合物と硬化触媒(硬化促進剤)とを併用
するというシステムが挙げられ、第二に、エポキシ樹脂
(A)のアニオン重合触媒能を有する、3級アミノ基含
有化合物または4級アンモニウム塩基含有化合物を用い
るというシステムが挙げられる。
As the curing agent system used in the present invention, to exemplify only typical ones, firstly, a curing agent system having an active hydrogen that can react with the epoxy group in the epoxy resin (A) as mentioned above is used. There are systems in which compounds containing primary and/or secondary amino groups are used as they are, or in combination with these amino group-containing compounds and a curing catalyst (curing accelerator). ) A system using a tertiary amino group-containing compound or a quaternary ammonium base-containing compound having an anionic polymerization catalytic ability can be mentioned.

上記した第一のシステムで用いられるアごノ基含有化合
物として特に代表的なもののみを挙げるに止めれば、ポ
リアルキレンボリア短ン、ポリアルキルエーテルボリア
ξン、ジシアンシア旦ド、ジヒドラジド類またはシアミ
ノジフェニルメタンの如き芳香族アミン化合物などであ
り、これらの使用量としては、活性水素/エポキシ基の
当量比が0.4 / 1.0〜1.2 / 1.0なる
範囲内が、好ましくは、0.6 / 1.0〜1.0 
/ 1.0なる範囲内が適切である。
Typical examples of the agono group-containing compounds used in the first system mentioned above include polyalkylene boria, polyalkyl ether boria, dicyanthyanide, dihydrazides, and cyamino These are aromatic amine compounds such as diphenylmethane, and the amount used thereof is preferably within a range where the active hydrogen/epoxy group equivalent ratio is 0.4/1.0 to 1.2/1.0. 0.6/1.0~1.0
/1.0 is appropriate.

かかる当量比が0.4よりも小さい場合には、どうして
も、充分な架橋密度のものが得られ難くなるので好まし
くないし、一方、1.2よりも大きい0 場合には、どうしても、未反応アミン分が多くなるので
好ましくない。
If the equivalent ratio is less than 0.4, it becomes difficult to obtain a sufficient crosslinking density, which is undesirable. On the other hand, if the equivalent ratio is more than 1.2, unreacted amine content inevitably increases. This is not desirable as it increases the number of

この第一のシステムの実施にさいしては、硬化触媒(硬
化促進剤)の併用は特に必要ではないけれども、併用し
うるものとして特に代表的なもののみを挙げるに止めれ
ば、1〜リス−(ジメチルアミノメチル)フェノール、
ジメチルヘンシルアミンまたはイミダゾールもしくはそ
の誘導体の如き各種の3級アミン類;ポリプロピレング
リコールまたはその誘導体の如き各種のアルコール類;
フェノール−ホルマリン縮合物の如き各種のフェノール
化合物;あるいは、サリチル酸またはスルホン酸系化合
物の如き各種の有機酸化合物などである。
When implementing this first system, it is not particularly necessary to use a curing catalyst (curing accelerator) in combination, but to list only typical ones that can be used in combination, dimethylaminomethyl)phenol,
various tertiary amines such as dimethylhensylamine or imidazole or its derivatives; various alcohols such as polypropylene glycol or its derivatives;
Various phenol compounds such as phenol-formalin condensates; or various organic acid compounds such as salicylic acid or sulfonic acid compounds.

そして、かかる硬化触媒(硬化促進剤)の使用量として
は、エポキシ樹脂(A)に対して2重量%以下が適当で
あり、2重量%を超える場合には、どうしても、耐水性
や可撓性が損われることになるので好ましくない。
The appropriate amount of the curing catalyst (curing accelerator) to be used is 2% by weight or less based on the epoxy resin (A), and if it exceeds 2% by weight, water resistance and flexibility will inevitably be This is not desirable because it will damage the

前述した第二のシステムにおいて用いられる含窒素化合
物として特に代表的なもののみを挙げる1 に止めれば、硬化触媒(硬化促進剤)の一種として上掲
された如き各種の3級アミン類;あるいは、テトラメチ
ルアンモニウムクロライドまたはテトラメチルアンモニ
ウムブロマイドの如き各種の4級アンモニウム塩類など
である。
Particularly representative nitrogen-containing compounds used in the second system mentioned above include: 1) various tertiary amines as listed above as a type of curing catalyst (curing accelerator); These include various quaternary ammonium salts such as tetramethylammonium chloride or tetramethylammonium bromide.

かかるアニオン重合触媒の使用量としては、エポキシ樹
脂(A)に対して5重量%以下が適当であり、好ましく
は、3重量%以下が適切である。
The amount of such anionic polymerization catalyst to be used is suitably 5% by weight or less, preferably 3% by weight or less, based on the epoxy resin (A).

5重量%を超えて多量に用いる場合には、硬化物の耐水
性が損われるようになるので好ましくない。
If it is used in a large amount exceeding 5% by weight, the water resistance of the cured product will be impaired, which is not preferable.

かくして得られる本発明の硬化性樹脂組成物には、さら
に必要に応じて、溶剤、無機質充填剤、顔料または難燃
剤などの公知慣用の各種の添加剤成分を、適宜、配合す
ることもできる。
The thus obtained curable resin composition of the present invention may further contain various known and commonly used additive components such as a solvent, an inorganic filler, a pigment, or a flame retardant, if necessary.

そのうち、無4a質充填剤として代表的なもののみを例
示するに止めれば、ジルコニウム粉末、石英ガラス粉末
、タルク粉末、炭酸カルシウム粉末、マグネシウム粉末
、珪酸カルシウム粉末またはシリカ粉末などである。
Among them, typical non-4a fillers include zirconium powder, quartz glass powder, talc powder, calcium carbonate powder, magnesium powder, calcium silicate powder, and silica powder.

2 そして、本発明組成物を硬化せしめるにさいしての、い
わゆる硬化温度としては80°C以上の温度が適当であ
り、要求される硬化時間に伴って、かかる硬化温度が、
適宜、選択されることになる。
2. When curing the composition of the present invention, a temperature of 80°C or higher is appropriate, and depending on the required curing time, the curing temperature may vary depending on the curing temperature.
It will be selected as appropriate.

〔発明の効果〕〔Effect of the invention〕

本発明の硬化性樹脂組成物は、とりわけ、硬化触媒ない
しは硬化促進剤の使用量の低減化が図りうるし、極力、
加熱硬化温度の低減化をも図りうるし、しかも、耐水性
および可撓性などにすぐれる硬化物を与えるものである
。
In particular, the curable resin composition of the present invention can reduce the amount of curing catalyst or curing accelerator used, and
The heat curing temperature can be lowered, and a cured product with excellent water resistance and flexibility can be obtained.

〔実施例〕〔Example〕

次に、本発明を参考例、実施例および比較例により、−
層、具体的に説明する。以下において、部および%は特
に断りのない限り、すべて重量基準であるものとする。
Next, the present invention will be explained by reference examples, examples, and comparative examples.
The layer will be explained in detail. In the following, all parts and percentages are based on weight unless otherwise specified.

参考例1 〔エポキシ樹脂(A)の調製例〕温度計、攪
拌機および加熱装置を備えた11のフラスコに、「エピ
クロン(EPICLON ) 850 j〔大日本イン
キ化学工業(株)製の、ビスフエノルA型エポキシ樹脂
;エポキシ当量−188g3 /eq)の772g、ビスフェノールAの128g。
Reference Example 1 [Example of Preparation of Epoxy Resin (A)] Into 11 flasks equipped with a thermometer, a stirrer, and a heating device, “EPICLON 850 J [bisphenol type A manufactured by Dainippon Ink and Chemicals Co., Ltd.] Epoxy resin; 772 g of epoxy equivalent (-188 g3/eq), 128 g of bisphenol A.

ビスフェノールSの100gおよび10%水酸化ナトリ
ウム水溶液の0.1gを仕込んで170℃に昇温し、同
温度に6時間のあいだ保持して反応を続行させた処、エ
ポキシ当量が506 g/eqで、150℃における溶
融粘度が24ボイズで、かつ、環球法による軟化点(以
下同様)が91℃なるエポキシ樹脂が得られた。
100 g of bisphenol S and 0.1 g of 10% aqueous sodium hydroxide solution were charged, the temperature was raised to 170°C, and the reaction was continued by holding at the same temperature for 6 hours, and the epoxy equivalent was 506 g/eq. An epoxy resin having a melt viscosity of 24 voids at 150°C and a softening point (the same applies hereinafter) of 91°C by the ring and ball method was obtained.

なお、このもののビスフェノールSの含有率は10%で
あった。
Note that the content of bisphenol S in this product was 10%.

参考例2(同上) 参考例1と同様のフラスコに、「エピクロンEXA−1
514J (同上社製の、ビスフェノールS型エポキシ
樹脂;エポキシ当量−310g/eq、ビスフェノール
S含有率−60%)の117g、「エピクロン850」
の642 g、ビスフェノールAの241gおよび10
%水酸化ナトリウム水溶液の0.1gを仕込んで190
℃に昇温し、同温度に4時間のあいだ保持して反応を続
行せしめた処、エポキシ当量が600g/eqで、15
0℃におけ4 る溶融粘度が40ポイズで、軟化点が90°Cで、かつ
、ビスフェノールS含有率が7%なるエポキシ樹脂(A
)が得られた。
Reference Example 2 (same as above) In a flask similar to Reference Example 1, “Epicron EXA-1
117 g of 514J (manufactured by the same company, bisphenol S type epoxy resin; epoxy equivalent - 310 g/eq, bisphenol S content - 60%), "Epicron 850"
642 g of bisphenol A, 241 g of bisphenol A and 10
190% by adding 0.1g of sodium hydroxide aqueous solution.
When the temperature was raised to ℃ and kept at the same temperature for 4 hours to continue the reaction, the epoxy equivalent was 600 g/eq and 15
An epoxy resin (A
)was gotten.

実施例1および2ならびに比較例1〜3第1表に示され
るような配合Mi戒に従って配合せしめて各種の硬化性
樹脂組成物を得た。
Examples 1 and 2 and Comparative Examples 1 to 3 Various curable resin compositions were obtained by blending according to the formulation guidelines shown in Table 1.

次いで、かくして得られたそれぞれの硬化性樹脂組成物
を塗料として用いて、格別に、厚さが2mlなるサンド
フ゛ラスト板または厚さが1.2uなる磨軟鋼板に、膜
厚が200ミクロンとなるように塗布しく但し、磨軟鋼
板はエリクセン値の測定の場合に限られる。)、140
℃で30分間のあいだ焼付けを行なって、各種の硬化塗
膜を得た。
Next, each of the curable resin compositions thus obtained was used as a coating material to coat a 2 ml thick sand blast board or a 1.2 u thick polished mild steel board so that the film thickness was 200 microns. However, the use of polished mild steel plates is limited to the measurement of Erichsen values. ), 140
Various cured coating films were obtained by baking at .degree. C. for 30 minutes.

しかるのち、それぞれの硬化塗膜について諸性能の比較
検討を行なった。それらの結果は同表に示す通りである
。
Thereafter, various performances of each cured coating film were compared and studied. The results are shown in the same table.

なお、それぞれの硬化性樹脂組成物について、140℃
に保持されたキュアープレー1〜上での「ゲルタイム」
の測定をも行なった。それらの結果も、併せて、同表に
示す。
In addition, for each curable resin composition, 140°C
"Gel Time" on Cure Play 1~ held in
We also conducted measurements. The results are also shown in the same table.

5 第1表を見ても明らかなように、本発明の硬化性樹脂1
lJl戒物は、低温での加熱硬化においても、可撓性や
耐湿性などにすぐれた硬化物を与えるものであることが
知れる。
5 As is clear from Table 1, curable resin 1 of the present invention
It is known that lJl Kaimono gives a cured product with excellent flexibility and moisture resistance even when heated and cured at low temperatures.

代 理 人teenager Reason Man

Claims (1)

【特許請求の範囲】 1、式 ▲数式、化学式、表等があります▼…〔 I 〕 なる繰り返し単位を主要構成単位として有する、4,4
′−ジヒドロキシジフェニルスルホンを必須の原料成分
として得られるエポキシ樹脂(A)と、アミン系エポキ
シ樹脂硬化剤(B)とを含んで成る、硬化性樹脂組成物
。 2、前記した式 ▲数式、化学式、表等があります▼…〔 I 〕 なる繰り返し単位を主要構成単位として有する、4,4
′−ジヒドロキシジフェニルスルホンを必須の原料成分
として得られるエポキシ樹脂(A)が、上記の4,4′
−ジヒドロキシジフェニルスルホンを3〜60重量%な
る範囲内で用いて得られるものである、請求項1に記載
の硬化性樹脂組成物。 3、前記したアミン系エポキシ樹脂硬化剤(B)が、エ
ポキシ基と反応しうる活性水素をもった1級、および/
または2級アミノ基を有する化合物である、請求項1に
記載の硬化性樹脂組成物。 4、前記したアミン系エポキシ樹脂硬化剤(B)が、前
記したエポキシ樹脂(A)のアニオン重合触媒機能をも
った、3級アミノ基または4級アンモニウム塩基を有す
る化合物である、請求項1に記載の硬化性樹脂組成物。
[Claims] 1. Formula ▲ There are mathematical formulas, chemical formulas, tables, etc. ▼…[I] Having a repeating unit as a main constituent unit, 4,4
A curable resin composition comprising an epoxy resin (A) obtained with '-dihydroxydiphenylsulfone as an essential raw material component and an amine-based epoxy resin curing agent (B). 2. The above-mentioned formula▲There are mathematical formulas, chemical formulas, tables, etc.▼...[I] Having the repeating unit as the main constituent unit, 4,4
Epoxy resin (A) obtained using '-dihydroxydiphenyl sulfone as an essential raw material component is the above-mentioned 4,4'
The curable resin composition according to claim 1, which is obtained by using 3 to 60% by weight of -dihydroxydiphenylsulfone. 3. The above-described amine-based epoxy resin curing agent (B) is a primary resin having an active hydrogen that can react with an epoxy group, and/
or a compound having a secondary amino group, the curable resin composition according to claim 1. 4. The above-mentioned amine-based epoxy resin curing agent (B) is a compound having a tertiary amino group or a quaternary ammonium base and having an anionic polymerization catalytic function of the above-mentioned epoxy resin (A). The curable resin composition described.
JP19915289A 1989-07-31 1989-07-31 Curing resin composition Ceased JPH0362820A (en)