JPH0363441B2 - - Google Patents
Info
- Publication number
- JPH0363441B2 JPH0363441B2 JP60038376A JP3837685A JPH0363441B2 JP H0363441 B2 JPH0363441 B2 JP H0363441B2 JP 60038376 A JP60038376 A JP 60038376A JP 3837685 A JP3837685 A JP 3837685A JP H0363441 B2 JPH0363441 B2 JP H0363441B2
- Authority
- JP
- Japan
- Prior art keywords
- striped
- rolling
- protrusions
- mill
- protrusion
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Lifetime
Description
【発明の詳細な説明】
<産業上の利用分野>
この発明は、コンクリート類との付着性能を高
めるためにフランジ外面に縞突起が設けられたH
形鋼あるいは類似形鋼の圧延方法に関するもので
ある。[Detailed Description of the Invention] <Industrial Application Field> The present invention is directed to an H flange in which striped protrusions are provided on the outer surface of the flange in order to improve adhesion performance with concrete.
This relates to a method of rolling steel sections or similar sections.
<従来技術とその問題点>
第10図に示すように、従来の縞成形は、ユニ
バーサル粗ミル(以下URミル)1の後段のユニ
バーサル仕上ミル(以下UFミル)2において1
パスで行なつていた。<Prior art and its problems> As shown in FIG.
I was doing it with a pass.
これはUFミル2の竪ロール3に縞孔型3Aを
形成し、1パスで縞突起4を浮き上げる縞成形法
であり、高い縞突起4を得ようとすると、突起高
さの倍以上、フランジ厚を圧下することが必要で
ある。このため、UFミルの竪ロール圧延荷重は
通常のH形鋼時200〜300トンであるのに対し、2
mmの突起を得るのでさえ400トン以上かかり、通
常のミル設備からいつて2mmが最高であつた。 This is a stripe forming method in which a striped hole type 3A is formed on the vertical roll 3 of the UF mill 2 and the striped protrusions 4 are raised in one pass. It is necessary to reduce the flange thickness. For this reason, the vertical roll rolling load of the UF mill is 200 to 300 tons for normal H-beam steel, but
It took more than 400 tons to even obtain a millimeter protrusion, and the maximum was 2 mm using normal mill equipment.
一方、フランジを4mm以上圧下すると材料の出
側速さV0とロールの周速V1の差が大きくなり
(V0>V1)、先進率φ=(V0/V1)−1も大きくな
る。 On the other hand, when the flange is rolled down by 4 mm or more, the difference between the exit speed V 0 of the material and the circumferential speed V 1 of the roll increases (V 0 > V 1 ), and the advance rate φ = (V 0 /V 1 )-1 also increases. growing.
このφが大きくなると材料が孔型よりも速く進
むため、孔型に充満していた突起は、逆に孔型で
削り取られるようになり、突起の起き上がり角度
が45゜以下のかなり滑らかなものになつてしまう
(第8図参照)。 When this φ increases, the material advances faster than the hole mold, so the protrusions that were filling the hole mold are instead scraped away by the hole mold, and the rising angle of the protrusions becomes quite smooth with less than 45 degrees. I get used to it (see Figure 8).
そのため、現状のミル能力で従来より数倍の突
起高さが得られ、さらには、先進率を非常に小さ
くすることにより突起の起き上がり角度を60゜以
上にすることが可能な縞付きH形鋼の圧延方法
を、本発明者は既に開発し出願している(特願昭
58−226638号公報)。 Therefore, with the current milling capacity, it is possible to obtain a protrusion height several times that of conventional methods, and by making the advance rate extremely small, it is possible to make the protrusion rise angle over 60° with striped H-beam steel. The inventor has already developed and applied for a rolling method (patent application
58-226638).
これは第11図に示すように、URミル1にお
いて、各パスごとの材料フランジ幅をほぼ一定に
保持する往復圧延により、フランジ外面に圧延方
向に延在し、幅方向に多条の突条5を形成し、続
いて、この突条5をUFミル2の竪ロール6によ
り圧延方向に断続的に圧下して縞突起7を形成す
るようにしたものである。 As shown in Fig. 11, in the UR mill 1, by reciprocating rolling that keeps the material flange width approximately constant for each pass, many protrusions are formed on the outer surface of the flange in the rolling direction and in the width direction. 5 is formed, and then this protrusion 5 is intermittently rolled down in the rolling direction by a vertical roll 6 of the UF mill 2 to form striped protrusions 7.
この竪ロール6は、実際には第12図に示すよ
うに、ロール外周面に等間隔をおいて幅方向に沿
うスリツト溝8を穿設した構成であり、幅方向の
拘束がないため、突条5を分断圧下すると突起が
幅方向に流れて第13図に示すような形状7′と
なり、形状不良により付着性能が低下し、製品と
しての外観体裁が悪くなるなどの問題点が生じ
る。 As shown in FIG. 12, this vertical roll 6 actually has a structure in which slit grooves 8 are formed along the width direction at equal intervals on the roll outer circumferential surface, and there is no restriction in the width direction, so there are no projections. When the strip 5 is divided and rolled down, the protrusions flow in the width direction to form a shape 7' as shown in FIG. 13, which causes problems such as poor shape, poor adhesion performance, and poor appearance as a product.
この発明はこのような問題点を解消すべく提案
されたもので、その目的は、比較的縞高さが高
く、かつ突起の起き上がり角度の大きく、さらに
形状不良なく高品質な縞突起を比較的小さな圧延
荷重で成形し得る縞付形鋼の圧延方法を提供する
ことにある。 This invention was proposed to solve these problems, and its purpose is to produce relatively high-quality striped protrusions that have a relatively high stripe height, a large rising angle of the protrusions, and are free from poor shape. An object of the present invention is to provide a method for rolling striped section steel that can be formed with a small rolling load.
<問題点を解決するための手段>
この発明に係る縞付形鋼の圧延方法は、表面に
多数の縞突起を有する縞付形鋼の圧延方法であつ
て、URミルなどの前段ミルにより圧延方向に連
続する突条を形成し、引き続きロール外周に前記
縞突起に対応した多数の縞孔型を刻設した後段圧
延機により、前記連続突条を分断するとともに該
分断余肉を前記縞孔型内に充満させて縞突起を形
成させるようにしたものである。<Means for Solving the Problems> The method for rolling a striped section steel according to the present invention is a method for rolling a striped section steel having a large number of striped projections on the surface, and is a method for rolling a striped section steel having a large number of striped projections on the surface. After forming continuous protrusions in the direction, a subsequent rolling mill in which a large number of striped holes corresponding to the striped protrusions is carved on the outer periphery of the roll is used to divide the continuous protrusions and cut the separated excess into the striped holes. It fills the mold to form striped protrusions.
<実施例>
以下この発明を図示する一実施例に基づいて説
明する。<Example> The present invention will be described below based on an illustrated example.
第1図に示すように、2条の孔型9Aが穿設さ
れたURミル1の竪ロール9によりH形鋼のフラ
ンジ外面に圧延方向に連続し幅方向に2条の突条
10を形成し、続いてロール外周に縞突起11に
対応した2条で多数の縞孔型12Aを設けたUF
ミル2の竪ロール12により1パスで突条10を
分断するとともに縞孔型12Aに充満させて縞突
起11を得る。 As shown in Fig. 1, two protrusions 10 are formed on the outer surface of the flange of the H-section steel in the rolling direction and in the width direction by the vertical roll 9 of the UR mill 1, which has two grooves 9A. Then, a UF with a large number of striped holes 12A in two stripes corresponding to the striped protrusions 11 is provided on the outer periphery of the roll.
The vertical roll 12 of the mill 2 divides the protrusion 10 in one pass and fills the striped hole mold 12A to obtain the striped protrusion 11.
URミル1では複数回のリバース圧延で、孔型
9Aと突条10とがずれないようにフランジ幅を
ほぼ一定に保持して行ない、これにより高さ5〜
10mmと突条10を安定して得ることができる。な
お、これに限らず1パスで突条10を成形するこ
とも可能である。 In the UR mill 1, reverse rolling is performed multiple times while keeping the flange width almost constant so that the groove 9A and the protrusion 10 do not shift.
10mm and protrusion 10 can be stably obtained. Note that the present invention is not limited to this, and it is also possible to form the protrusions 10 in one pass.
UFミル2では、縞孔型12Aの幅を孔型9A
の幅とほぼ等しくするとともに縞孔型12Aと1
2Aとの間隔は突条10の高さと縞突起11の高
さとにより適宜設定される。 In UF Mill 2, the width of striped hole type 12A is changed to hole type 9A.
The width of the striped hole type 12A and 1
2A is appropriately set depending on the height of the protrusion 10 and the height of the striped protrusion 11.
以上のような構成において、突条10を縞孔型
12Aにより分断するとともにこの孔型12A内
に充満させるため、比較的小さい圧延荷重で縞突
起11を十分に高くでき、さらに材料先進率を減
少させることができ縞突起11の起き上がり角度
を大とすることができる。 In the above configuration, since the protrusions 10 are divided by the striped holes 12A and the holes 12A are filled, the striped protrusions 11 can be made sufficiently high with a relatively small rolling load, and the material advance rate can be further reduced. Therefore, the rising angle of the striped protrusions 11 can be increased.
なお、圧延時にURミル1、UFミル2の一方、
もしくは両方に圧延油を供給して縞成形を容易に
してもよい。また、製品の搬送に際して冷却、矯
正、検査、パイリングをフランジを上下として行
なうのでなく、H形で処理するようにし縞突起1
1の変形を防止するようにしてもよい。 In addition, during rolling, one of UR mill 1 and UF mill 2,
Alternatively, rolling oil may be supplied to both to facilitate stripe forming. In addition, when transporting products, cooling, straightening, inspection, and piling are not performed with the flanges above and below, but are processed in an H shape, so that striped protrusions 1
1 may be prevented from deforming.
また、図では2条としたがこれに限らず1条で
も多条でもよい。 Further, although the figure shows two threads, the present invention is not limited to this, and it may be one thread or multiple threads.
<具体例>
本発明に係る圧延方法により縞高さ3.5mm以上
で縞起き上がり角60゜以上の縞突起11を有し第
4図ないし第6図に示すような形状の縞付きH形
鋼をH300×200、H400×200、H450×200、
H500×200、H600×200の5シリーズにわたつて
製造した。<Specific Example> By the rolling method according to the present invention, a striped H-shaped steel having a striped protrusion 11 with a stripe height of 3.5 mm or more and a stripe rise angle of 60° or more and a shape as shown in FIGS. 4 to 6 is produced. H300×200, H400×200, H450×200,
Five series were manufactured: H500×200 and H600×200.
その結果、UFミル2で得られる縞高さhと、
その時のフランジ圧下率ln(tfo/tff)の関係は、
第7図で示すように、次の回帰式で求められる。 As a result, the stripe height h obtained with UF Mill 2,
The relationship between the flange reduction rate ln (tfo/tff) at that time is:
As shown in FIG. 7, it is determined by the following regression equation.
ln(tfo/tff)≧α・(h/tfo)2/3
また、フランジ圧下率と材料先進率との関係は
第8図に示すようになり、同じ圧下率の場合に
は、明らかに従来の圧延方法に比べて先進率が減
少することがわかる。この材料先進率の大幅低下
により縞突起の圧延トツプ側の起き上がり角度は
大幅に改善された。 ln(tfo/tff)≧α・(h/tfo) 2/3 Furthermore, the relationship between the flange reduction rate and the material advance rate is as shown in Figure 8, and when the same reduction rate is used, it is clear that It can be seen that the advance rate is reduced compared to the rolling method. Due to this significant reduction in the material advancement rate, the rising angle of the striped protrusions on the rolling top side was significantly improved.
これにより縞高さ最大6mm、縞起き上がり角度
最大70゜の縞成形が可能であることを明らかとな
つた。 This revealed that it is possible to form stripes with a maximum stripe height of 6 mm and a maximum stripe rise angle of 70°.
なお、以上はH形鋼について説明したが、これ
に限らず山形鋼などその他の類似形鋼にも本発明
を適用できることはいうまでもない。 Although the above description has been made regarding H-shaped steel, it goes without saying that the present invention is not limited to this and can be applied to other similar shaped steels such as angle-shaped steel.
<発明の効果>
前述のとおりこの発明によれば前段ミルで成形
された突条を縞孔型により分断するとともにこの
孔型内に充満させるようにしたため、次のような
効果を奏する。<Effects of the Invention> As described above, according to the present invention, the protrusions formed in the former stage mill are divided by the striped holes and the holes are filled, so that the following effects are achieved.
() 縞高さが高く、縞起き上がり角度の大きい
縞突起を得ることができる。() It is possible to obtain striped protrusions with a high stripe height and a large stripe rise angle.
() 幅方向にも拘束のある縞孔型による充満圧
延であるため形状不良がなく()と相まつて
コンクリート類との付着性能が良い。() Since it is filled rolling using a striped hole type with constraints in the width direction, there is no shape defect and combined with (), it has good adhesion performance with concrete.
() UFミルの圧下率、圧延荷重の減少を図る
ことができる。() It is possible to reduce the rolling reduction rate and rolling load of the UF mill.
() 縞成形用の竪ロールの寿命、ロール原単位
の向上を図れる。() It is possible to improve the life of vertical rolls for stripe forming and the roll consumption rate.
第1図はこの発明に係る圧延方法を実施するた
めの圧延機列を示す斜視図、第2図はそのUFミ
ルの竪ロールを示すロール表面展開図、第3図は
本発明に係る縞付H形鋼を示す斜視図、第4図、
第5図は同様のH形鋼を示す断面図、平面図、第
6図はその縞突起の拡大平面図、第7図は縞高さ
とフランジ圧下率との関係を示すグラフ、第8図
は縞角度とフランジ先進率の関係を示す概略図、
第9図はフランジ圧下率と材料先進率の関係を示
すグラフ、第10図は従来の圧延方法を実施する
ための圧延機列を示す斜視図、第11図はもう一
つの従来例を示す斜視図、第12図はそのUFミ
ルの竪ロールを示すロール表面展開図、第13図
はこのロールにより成形された従来の縞付H形鋼
を示す斜視図である。
1……URミル、2……UFミル、3……竪ロ
ール、3A……縞孔型、4……縞突起、5……突
条、6……竪ロール、7,7′……縞突起、8…
…スリツト溝、9……竪ロール、9A……孔型、
10……突条、11……縞突起、12……竪ロー
ル、12A……縞孔型。
FIG. 1 is a perspective view showing a rolling mill row for carrying out the rolling method according to the present invention, FIG. 2 is a developed view of the roll surface showing the vertical rolls of the UF mill, and FIG. 3 is a striped rolling mill according to the present invention. A perspective view showing an H-beam, Figure 4.
Fig. 5 is a cross-sectional view and a plan view showing a similar H-section steel, Fig. 6 is an enlarged plan view of its striped protrusions, Fig. 7 is a graph showing the relationship between stripe height and flange reduction ratio, and Fig. 8 is a graph showing the relationship between stripe height and flange reduction ratio. Schematic diagram showing the relationship between fringe angle and flange advance rate,
Fig. 9 is a graph showing the relationship between the flange reduction rate and the material advance rate, Fig. 10 is a perspective view showing a row of rolling mills for carrying out the conventional rolling method, and Fig. 11 is a perspective view showing another conventional example. 12 is a roll surface developed view showing the vertical roll of the UF mill, and FIG. 13 is a perspective view showing a conventional striped H-section steel formed by this roll. 1...UR mill, 2...UF mill, 3...Vertical roll, 3A...Striped hole type, 4...Striped protrusion, 5...Protrusion, 6...Vertical roll, 7,7'...Striped Protrusion, 8...
...slit groove, 9...vertical roll, 9A...hole shape,
10...Protrusion, 11...Striped protrusion, 12...Vertical roll, 12A...Striped hole type.
Claims (1)
方法において、圧延材のすくなくとも一面に、前
段の圧延機により圧延方向に連続する突条を形成
し、引き続きロール外周に前記縞突起に対応した
多数の縞孔型を刻設した後段圧延機により、前記
連続突条を分断するとともに該分断余肉を前記縞
孔型内に充満させて縞突起を形成させることを特
徴とする縞付形鋼の圧延方法。1. In a method of rolling a striped section steel having a large number of striped projections on the surface, a rolling mill in the previous stage forms a continuous protrusion in the rolling direction on at least one surface of the rolled material, and then the outer periphery of the roll corresponds to the striped projections. The striped shape is characterized in that the continuous protrusions are divided by a subsequent rolling mill in which a large number of striped holes are carved, and the separated extra thickness is filled in the striped holes to form striped protrusions. Steel rolling method.