JPH0424924A - Forming method for molybdenum film - Google Patents

Forming method for molybdenum film

Info

Publication number
JPH0424924A
JPH0424924A JP2124075A JP12407590A JPH0424924A JP H0424924 A JPH0424924 A JP H0424924A JP 2124075 A JP2124075 A JP 2124075A JP 12407590 A JP12407590 A JP 12407590A JP H0424924 A JPH0424924 A JP H0424924A
Authority
JP
Japan
Prior art keywords
film
molybdenum
gas
deposited
sputtering
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP2124075A
Other languages
Japanese (ja)
Other versions
JP3046829B2 (en
Inventor
Nobuhiko Tsunoda
信彦 角田
Tsutomu Wada
力 和田
Kinya Kato
加藤 謹矢
Hiroshi Saito
浩 斎藤
Yasuhiro Ukai
育弘 鵜飼
Kiyoshi Taruda
樽田 清
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hosiden Corp
NTT Inc
Original Assignee
Hosiden Corp
Nippon Telegraph and Telephone Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hosiden Corp, Nippon Telegraph and Telephone Corp filed Critical Hosiden Corp
Priority to JP2124075A priority Critical patent/JP3046829B2/en
Priority to US07/697,991 priority patent/US5162933A/en
Priority to KR1019910007935A priority patent/KR950002943B1/en
Priority to EP91107967A priority patent/EP0457328B1/en
Priority to DE69116218T priority patent/DE69116218T2/en
Publication of JPH0424924A publication Critical patent/JPH0424924A/en
Application granted granted Critical
Publication of JP3046829B2 publication Critical patent/JP3046829B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

PURPOSE:To modify columnar composition of a sputter molybdenum film and to form a molybdenum film in which a lower layer material is not corroded and not damaged by depositing the film by using sputter gas mixed with nitrogen gas. CONSTITUTION:An ITO 2 is deposited 500Angstrom on a glass board 1, nitrogen gas is mixed by 10% with argon used as sputter gas, and a molybdenum nitride film 4 is deposited 1000Angstrom . A molybdenum target containing a purity of 99.9wt.% or higher is used. The sputter gas is mixture gas of argon 27SCCM and N2 gas 3SCCM, its pressure is 3.0mTorr, sputter power is 2.0A of constant current, a voltage is about 500V, 1kw, and the moving speed of the board is 120mm/min. Then, the film 4 of 1000Angstrom is deposited. The molybdenum nitride film deposited by the N2 mixture 10% sputter gas does not corrode and not damage the ITO.

Description

【発明の詳細な説明】 〔産業上の利用分野〕 本発明はモリブデン膜の形成方法に関し、さらに詳しく
は薄膜形成技術を用いて作製されるLSI、液晶表示パ
ネル等の電子デバイスにおけるモリブデン膜とアルミニ
ウム膜を積層した配線材料の形成方法に関する。
Detailed Description of the Invention [Field of Industrial Application] The present invention relates to a method for forming a molybdenum film, and more specifically to a method for forming a molybdenum film and aluminum in electronic devices such as LSIs and liquid crystal display panels manufactured using thin film forming technology. The present invention relates to a method for forming a wiring material in which films are laminated.

〔従来の技術〕[Conventional technology]

モリブデンは、高融点金属であるため耐熱性に優れ、ま
たケミカルウェットエツチングによる加工性も、他の高
融点金属に比べ比較的容易なこともあって、LSI等の
集積回路や、薄膜トランジスタを用いた薄膜デバイスの
電極材料や、配線材料として広く使用されている。
Molybdenum is a high melting point metal, so it has excellent heat resistance, and it is relatively easy to process using chemical wet etching compared to other high melting point metals, so it is used in integrated circuits such as LSIs and thin film transistors. It is widely used as an electrode material for thin film devices and as a wiring material.

しかし、通常のアルゴンガスを用いて、モリブデンをス
パッタ法で堆積成膜すると、基板に垂直な柱状組織に形
成されることが知られている。したがって、モリブデン
のスパッタ膜をケミカルウェットエツチング加工でバタ
ン形成すると、柱状組織構造を転写して寸法精度は高い
が、バタン端の形状が垂直となり、この垂直側壁が上層
での配線の断線や絶縁膜の耐圧不足による短絡の起因と
なる欠点があった。
However, it is known that when molybdenum is deposited by sputtering using ordinary argon gas, a columnar structure is formed perpendicular to the substrate. Therefore, when a molybdenum sputtered film is formed into a batten by chemical wet etching, the columnar structure is transferred and the dimensional accuracy is high, but the shape of the batten edge becomes vertical, and these vertical sidewalls cause disconnection of wiring in the upper layer and insulating film. This had the disadvantage of causing short circuits due to insufficient withstand voltage.

さらに、柱状組織であること、スパッタという低温成膜
のために組織の結合性が脆弱であることから、ホトリソ
グラフィ処理や、ケミカルウェットエツチング処理中に
現像液やエツチング液が膜厚方向に、すなわち、柱状組
織に沿って浸入し易く下層の材料を損傷する欠点があっ
た。例えば、LCD (液晶素子)用アクティブマトリ
クスでは、配線の低抵抗化をはかる目的で透明電極のI
TO(インジウムとスズの酸化物よりなる透明電極)上
にAQ (アルミニウム)を重ねた積層構造を採用した
いところであるが、ITOとAQを直接重ねると、ケミ
カルウェットエツチングでのパタニングの際、異種金属
間の電池作用によってITOの優先的溶解による腐食が
生じる問題があった。
Furthermore, because the structure is columnar and the bonding of the structure is weak due to low-temperature film formation by sputtering, the developer or etching solution may be applied in the film thickness direction during photolithography or chemical wet etching. However, it has the disadvantage of easily penetrating along the columnar structure and damaging the underlying material. For example, in active matrices for LCDs (liquid crystal devices), the I
I would like to adopt a laminated structure in which AQ (aluminum) is layered on TO (a transparent electrode made of indium and tin oxide), but if ITO and AQ are layered directly, dissimilar metals will be removed during patterning using chemical wet etching. There was a problem in that corrosion occurred due to preferential dissolution of ITO due to battery action during the process.

ITOとAfiの中間にモリブデンを介在させるとIT
Oの腐食損傷は防止できるが、柱状組織のスパッタモリ
ブデン膜では、現像液やAQエツチング液の浸み込みが
生じ易<ITOが損傷されることがあり、完全にはIT
Oの腐食をなくすことができない欠点があった9さらに
、燐酸に小量の硝酸を添加したAQエツチング液を用い
てAQとモリブデンの積層膜をエツチング加工すると、
モリブデンのエツチング速度がAQよりも非常に大きい
ために、断面形状が下層のモリブデンがサイドエツチン
グされオーバハングが生じるという別の問題が発生した
。
When molybdenum is interposed between ITO and Afi, IT
Although O corrosion damage can be prevented, a sputtered molybdenum film with a columnar structure is easily penetrated by developer and AQ etching solution.
9 Furthermore, when a laminated film of AQ and molybdenum was etched using an AQ etching solution containing a small amount of nitric acid added to phosphoric acid,
Since the etching rate of molybdenum was much higher than AQ, another problem occurred in that the molybdenum in the lower layer of the cross-sectional shape was side-etched, resulting in overhang.

〔発明が解決しようとする課題〕[Problem to be solved by the invention]

上述したごとく、従来技術においては、モリブデン膜が
柱状組織であるためにバタン形成においてその端部の形
状が垂直となるため、この上層に設ける配線層の断線や
絶縁膜の耐圧不足による短絡が生じたり、またケミカル
ウェットエツチング処理中に、エツチング液がモリブデ
ン膜の柱状組織中に浸入し、下層の材料を腐食損傷させ
たり、さらに下層に設けたモリブデン膜のエツチング速
度が非常に大きいためにオーバハングが生じ易いなどの
問題があった。
As mentioned above, in the conventional technology, since the molybdenum film has a columnar structure, the end shape of the molybdenum film becomes vertical when forming the batten, resulting in disconnections in the wiring layer provided on the upper layer and short circuits due to insufficient withstand voltage of the insulating film. In addition, during the chemical wet etching process, the etching solution may penetrate into the columnar structure of the molybdenum film, corroding and damaging the underlying material.Furthermore, the etching rate of the underlying molybdenum film is extremely high, resulting in overhang. There were problems such as easy to occur.

本発明の目的は、上記従来技術における問題点を解消す
るものであって、スパッタモリブデン膜の柱状組織を改
質して、ケミカルウェットエツチングにおける下層材料
の腐食損傷ならびに下層モリブデン膜のサイドエツチン
グの生じないモリブデン膜の形成方法を提供するもので
あり、さらに具体的には、バタン断面がテーパ加工でき
、エツチング液などの浸み込みがなく、AQエツチング
液でのエツチング速度がAQとほぼ同程度以下のモリブ
デン膜を、スパッタ法により形成させる方法を提供する
ことにある。
An object of the present invention is to solve the above-mentioned problems in the prior art, and to improve the columnar structure of a sputtered molybdenum film to prevent corrosion damage to the underlying material and side etching of the underlying molybdenum film during chemical wet etching. More specifically, it provides a method for forming a molybdenum film that does not require etching.More specifically, the cross section of the batten can be tapered, there is no penetration of etching liquid, and the etching speed with AQ etching liquid is approximately the same or lower than that of AQ. An object of the present invention is to provide a method for forming a molybdenum film by sputtering.

〔課題を解決するための手段〕[Means to solve the problem]

上記本発明の目的は、スパッタ法によってモリブデン膜
とアルミニウム膜とを積層して積層膜を形成させる場合
に、上記モリブデン膜の形成において、窒素ガスを混合
したスパッタガスを用いてモリブデン膜を堆積させるこ
とにより達成される。
The object of the present invention is to deposit a molybdenum film using a sputtering gas mixed with nitrogen gas when forming a laminated film by laminating a molybdenum film and an aluminum film by sputtering. This is achieved by

さらに、本発明のモリブデン膜の形成方法において、ス
パッタガス中への窒素ガスの混合比を、モリブデン膜の
成長段階に応じて低減させながらモリブデン膜の堆積を
行うことがより好ましい。
Furthermore, in the method for forming a molybdenum film of the present invention, it is more preferable to deposit the molybdenum film while reducing the mixing ratio of nitrogen gas in the sputtering gas depending on the growth stage of the molybdenum film.

〔作   用〕[For production]

モリブデン膜の形成には、一般にはスパッタガスとして
アルゴンを用いるが、窒素ガスをスパッタガスであるア
ルゴンに混合してモリブデン膜を成膜したところ、エツ
チング速度が低下することが分かった。窒素ガスの混合
比とエツチング速度の関係を第1図に示す。燐酸を主成
分とした一般的なAQエツチング液では、窒素ガスを2
0%混合するとエツチング速度がアルゴン100%の場
合と比較して1/4になる。
Generally, argon is used as a sputtering gas to form a molybdenum film, but when a molybdenum film was formed by mixing nitrogen gas with argon, which is a sputtering gas, it was found that the etching rate decreased. FIG. 1 shows the relationship between the nitrogen gas mixing ratio and the etching rate. A general AQ etching solution containing phosphoric acid as its main component uses 2 nitrogen gases.
When argon is mixed at 0%, the etching rate becomes 1/4 of that when argon is mixed at 100%.

一方、エツチングによるバタン側壁の形状は、窒素ガス
の混合比が増加するにしたがい90度に近かったテーパ
角が低減し、窒素ガス20%の混合比で等方性エツチン
グの45度には至らなかったが50度程度になることが
分かった。
On the other hand, as for the shape of the batten side wall formed by etching, as the nitrogen gas mixture ratio increases, the taper angle, which was close to 90 degrees, decreases, and at a nitrogen gas mixture ratio of 20%, it does not reach the 45 degrees of isotropic etching. It turned out that the temperature was about 50 degrees.

スパッタガスであるアルゴンに窒素ガスを混合すること
によって現われる上述の現象は、スパッタガス中に窒素
が存在することで、モリブデンのスパッタ粒子がプラズ
マ中で窒化されて窒化モリブデン膜として堆積し、その
組織構造は柱状から均質構造へと窒素ガス混合比の増加
と共に進行し、膜組織が緻密化される結果と考えられる
。
The above-mentioned phenomenon that appears when nitrogen gas is mixed with argon, which is the sputtering gas, is due to the presence of nitrogen in the sputtering gas, which causes molybdenum sputtered particles to be nitrided in the plasma and deposited as a molybdenum nitride film. This is thought to be the result of the structure progressing from a columnar structure to a homogeneous structure as the nitrogen gas mixing ratio increases, and the film structure becomes denser.

本発明は上記現象に基づくもので、スパッタモリブデン
膜の成膜中にスパッタガスであるアルゴンに窒素ガスを
混入したことを特徴とし、エツチングによる断面をテー
パ状にすることを可能にし、下地へのエツチング液の浸
入を防ぎ、さらにはエツチング速度がAnと同等以下に
なってAQを重ねた積層膜のオーバハングのないエツチ
ング加工を可能とするモリブデン膜の形成方法を実現す
るものである。
The present invention is based on the above phenomenon, and is characterized in that nitrogen gas is mixed into argon, which is a sputtering gas, during the formation of a sputtered molybdenum film, making it possible to make the cross section tapered by etching, and to prevent the formation of a sputtered molybdenum film. The purpose of the present invention is to realize a method for forming a molybdenum film that prevents the infiltration of an etching solution, and further reduces the etching rate to the same or lower than that of An, thereby enabling etching of a laminated film of AQ without overhanging.

〔実施例〕〔Example〕

以下に本発明の実施例を挙げ、図面を参照しながらさら
に詳細に説明する。
Embodiments of the present invention will be described below in more detail with reference to the drawings.

実施例 1 ガラス基板(コーニング社製#7059)に。Example 1 on a glass substrate (Corning #7059).

ITOを200℃加熱の直流マグネトロンスパッタ法に
て500人堆積した試料基板を用いて、スパッタガスと
して用いたアルゴンに窒素(N2)ガスを10%混合し
て窒化モリブデン膜を1000人堆積した。スパッタ装
置は、ターゲット上50III11の位置に試料をセッ
トしたキャリアが移動して成膜するスパッタアップ方式
のものを用いた。モリブデンターゲットは、5インチ(
12,7dll)X15インチ(38,1cm)のサイ
ズで、99.9重量%以上の純度のものを使用した。試
料の加熱は、100℃でスパッタ中にも背面より加熱し
て保温した。スパッタガスはアルゴン275 CCM 
(Nad/win) 、N2ガスは3SCCMの混合ガ
スで圧力は3.0mTorr (ミリトル)とした。ス
パッタ電力は2.OAと電流−定力式で、電圧は約50
0Vで1kWとした。この条件で、基板の移動速度を1
20 am/l1inにすると1000人の窒化モリブ
デン膜が堆積された。
A molybdenum nitride film was deposited by 1000 people using a sample substrate on which 500 ITO was deposited by direct current magnetron sputtering method heated at 200° C. using a mixture of 10% nitrogen (N2) gas and argon used as a sputtering gas. The sputtering apparatus used was of a sputter-up type in which a carrier with a sample set at a position 50III11 above the target moved to form a film. The molybdenum target is 5 inches (
The sample used had a size of 12.7 dll) x 15 inches (38.1 cm) and a purity of 99.9% by weight or more. The sample was heated at 100° C. and kept warm by heating from the back side even during sputtering. Sputter gas is argon 275 CCM
(Nad/win), N2 gas was a mixed gas of 3SCCM and the pressure was 3.0 mTorr (mitorr). The sputtering power is 2. OA and current-constant force formula, voltage is approximately 50
It was set to 1kW at 0V. Under these conditions, the moving speed of the substrate is set to 1
At 20 am/l1in, 1000 molybdenum nitride films were deposited.

引き続き、同じスパッタ装置でAQを2000人堆積し
た。AQのスパッタ条件は、アルゴン305CCMで3
.0mTorr、スパッタ電力は6、OAの3kW、移
動速度は120 m/win。
Subsequently, 2000 AQ layers were deposited using the same sputtering equipment. AQ sputtering conditions are 305CCM of argon.
.. 0 mTorr, sputtering power 6, OA 3kW, and moving speed 120 m/win.

基板加熱は10.0℃とした。The substrate was heated to 10.0°C.

以上の条件で、ガラスウェハ基板上にITO(500人
)、窒化モリブデン(1000人)。
Under the above conditions, ITO (500 people) and molybdenum nitride (1000 people) were deposited on a glass wafer substrate.

Afl(2000人)が順に堆積した3層膜を形成した
。この構成は、LCDマトリクスの配線抵抗を低減させ
る場合のもので、ITOに直接AQを重ねた場合に生ず
る電池作用でのITOの腐食損傷を防ぐために用いられ
る。
A three-layer film was formed by sequentially depositing Afl (2000). This configuration is used to reduce the wiring resistance of the LCD matrix, and is used to prevent corrosion damage to ITO due to battery action that would occur if AQ was directly stacked on ITO.

配線パタンをウェットエツチングで加工形成するため、
ポジ型のホトレジスト(シブレイ社製マイクロポジット
1400−31)をスピンナで1.5虜塗布し、マスク
露光で所定の配線パタンを焼付け、2倍に薄めた現像液
(シブレイ社製MF−312)でシャワー現像した。こ
の現像液は、アミン系のかなり強度のアルカリ性で、従
来のスパッタガスとしてアルゴン100%で堆積したモ
リブデン膜では、現像時に下層のITOを損傷する障害
が発生する。その理由は、レジストが残らない領域、す
なわち配線部以外の領域では、AQ堆積膜のピンホール
等の欠陥や段差部上のAQ、の粗雑部分から浸入した現
像液が、柱状組織のモリブデン膜を通過して下層のIT
Oにまで到達し、AQとの電池作用で瞬間的に広範囲の
ITOを腐食させるためであると考えられる。
In order to process and form the wiring pattern by wet etching,
Apply 1.5 coats of positive photoresist (Microposit 1400-31 manufactured by Sibley) using a spinner, print the prescribed wiring pattern using mask exposure, and use a twice diluted developer (MF-312 manufactured by Sibley). I developed it in the shower. This developing solution is an amine-based and quite alkaline solution, and in the case of a molybdenum film deposited using 100% argon as a conventional sputtering gas, a problem occurs during development that damages the underlying ITO layer. The reason for this is that in areas where no resist remains, that is, areas other than wiring areas, the developer that has entered through defects such as pinholes in the AQ deposited film or rough areas of the AQ on the stepped portions can damage the columnar structure of the molybdenum film. through the underlying IT
It is thought that this is because the ITO reaches O and instantly corrodes a wide range of ITO due to the battery action with AQ.

本発明によるN2混合(本実施例の場合は10%)スパ
ッタガスで堆積した窒化モリブデン膜では、現像でのI
TOの腐食損傷は発生しなかった。
In the molybdenum nitride film deposited with the N2 mixed (10% in this example) sputtering gas according to the present invention, the I
No corrosion damage to TO occurred.

さらに、希釈していない原液の現像液を用い試料のAQ
膜がほとんど溶解するまで浸漬してもITOの損傷は全
く認められず、モリブデンの窒化により膜組織が緻密化
されるITOの腐食損傷の防止に顕著な効果のあること
が分かった。
Furthermore, the AQ of the sample using an undiluted developer solution.
Even when the film was immersed until it was almost dissolved, no damage to the ITO was observed, and it was found that the film was significantly effective in preventing corrosion damage to the ITO, which is caused by the densification of the film structure due to molybdenum nitridation.

ホトレジストパターンを形成後、120℃10分のハー
ドベーク処理をして、燐酸:酢酸:硝酸=20 : 3
 : 1のエツチング液でAl1膜と窒化モリブデン膜
を連続してエツチング加工した。
After forming the photoresist pattern, a hard bake treatment was performed at 120°C for 10 minutes to form a phosphoric acid:acetic acid:nitric acid ratio of 20:3.
: The Al1 film and the molybdenum nitride film were successively etched using the etching solution No. 1.

このエツチング液程においても上述した現像液の侵入と
同様の理由から、従来のアルゴン100%で堆積したモ
リブデン膜の場合にはITOの腐食損傷がより高頻度に
生じたが、本実施例においてはITOの腐食損傷は、上
記現像液の場合と同様に皆無であった。
In this etching solution process, corrosion damage to ITO occurred more frequently in the case of the conventional molybdenum film deposited with 100% argon due to the same reason as the intrusion of the developer mentioned above, but in this example, corrosion damage occurred more frequently. There was no corrosion damage to ITO, as in the case of the above developer.

さらに断面を[6すると、従来のアルゴン100%では
、第2図に示すように、モリブデン膜3のサイドエツチ
ングによるオーバハングの形状となるが、N2ガスを1
0%混入した本実施例の窒化モリブデン膜4の場合には
、第3図に示1ごとく、窒化モリブデン(Mo、N)膜
4とAΩ膜5はスムーズに連続した傾斜となり、テーパ
升状のバタン断面が得られた。これは、N2の混合ガス
によってエツチング速度が低下して、ALI5のエツチ
ング速度に近づいたことと、膜組織力均質で#密化され
ていることを示す。本実施例ては、N3ガスの混合比が
10%のこともあって。
Furthermore, if the cross section is [6], with conventional 100% argon, an overhang shape is formed due to side etching of the molybdenum film 3, as shown in FIG.
In the case of the molybdenum nitride film 4 of this example containing 0%, the molybdenum nitride (Mo, N) film 4 and the AΩ film 5 form a smoothly continuous slope as shown in FIG. A batan cross section was obtained. This indicates that the etching rate was reduced by the N2 mixed gas and approached the etching rate of ALI5, and that the film structure was homogeneous and dense. In this example, the mixing ratio of N3 gas was 10%.

上記バタン断面のテーパ角は60度程度であったが、N
2混合比を増加すれば下層の窒化モリブデン膜4のテー
パ角をさらに低減させることが可併であることは言うま
でもない。
The taper angle of the cross section of the baton was about 60 degrees, but N
It goes without saying that if the mixing ratio of 2 is increased, the taper angle of the underlying molybdenum nitride film 4 can be further reduced.

実施例 2 ガラス基板(コーニング社製#7059)上にアルゴン
ガスにN2を20%混合したスパッタガスを用いて窒化
モリブデンを1000人堆積したスパッタ装置は実施例
1の場合と同様の直流マグネトロンによるスパッタアッ
プ方式を用いた。モリブデンターゲットも実施例1と同
様の5インチX15インチサイズで99.9%以上の純
度のものを使用した。試料の加熱温度は100℃とし、
スパッタ中も加熱保温した。スパッタガスは、アルゴン
24SCCM、NN26SCCで3.0mTorrとし
た。スパッタ電力は2.OAの500Vで1kWとした
。キャリア移動速度を120 mn/winとして10
00人の窒化モリブデンをガラス基板上に堆積した後、
連続してスパッタガスをアルゴン100%に変更して、
窒化モリブデン上にモリブデン膜を1000人堆積した
ぁスパッタ条件は、アルゴンガス30 S CCMで3
.0mTorr、電力は2.OAの400■で800W
とした。この窒化モリブデンとモリブデンの2層の積層
膜に、ポジ型レジストで配線バタンを描き、燐酸:酢酸
:硝酸=20:3:1のエツチング液を用いてエツチン
グ加工した。配線パタンの断面形状を、SEM (走査
電子顕微鏡)で観察すると第4図に示すごとく、下層の
窒化モリブデン膜4はテーパエツチングされ、上層のモ
リブデン膜3は、はぼ垂直に近い形状となった。この積
層膜の電気抵抗は、シート抵抗から換算すると2.8X
10−’Ω・1であった。一方、N2ガスを20%混合
してスパッタした窒化モリブデン膜だけの場合は7.0
X10−’Ω・国となるので、2層構造によって抵抗を
172以下に低減させることができた。
Example 2 1000 molybdenum nitrides were deposited on a glass substrate (#7059 manufactured by Corning) using a sputtering gas containing 20% N2 mixed with argon gas.The sputtering equipment was the same as in Example 1, using direct current magnetron sputtering. The up method was used. The molybdenum target had the same size of 5 inches x 15 inches as in Example 1 and had a purity of 99.9% or more. The heating temperature of the sample was 100℃,
It was heated and kept warm during sputtering. The sputtering gas was 24SCCM of argon and 26SCC of NN at 3.0 mTorr. The sputtering power is 2. It was set to 1kW at 500V of OA. 10 assuming the carrier movement speed is 120 mn/win
After depositing 00 molybdenum nitride on the glass substrate,
Continuously change the sputtering gas to 100% argon,
A molybdenum film was deposited on molybdenum nitride by 1000 people.The sputtering conditions were 30 S CCM of argon gas.
.. 0mTorr, power is 2. OA's 400■ 800W
And so. Wiring patterns were drawn on this two-layer laminated film of molybdenum nitride and molybdenum using a positive resist, and etched using an etching solution containing phosphoric acid:acetic acid:nitric acid=20:3:1. When the cross-sectional shape of the wiring pattern was observed with an SEM (scanning electron microscope), as shown in Fig. 4, the lower layer molybdenum nitride film 4 was tapered etched, and the upper layer molybdenum film 3 had a nearly vertical shape. . The electrical resistance of this laminated film is 2.8X when converted from sheet resistance.
It was 10-'Ω·1. On the other hand, in the case of only a molybdenum nitride film sputtered with a mixture of 20% N2 gas, 7.0
Since the resistance becomes X10-'Ω·country, the resistance can be reduced to 172 or less by using the two-layer structure.

本実施例の結果から、スパッタガス中へのN2ガスの混
合比率を制御することで、配線抵抗の増加を抑制しなが
らエツチング加工でバタン断面のテーパ角を付は得るこ
とが可能となる。すなわち、本発明によればスパッタ膜
堆積の初期にはスパッタガス中へのN2ガス混合比を高
くし、スパッタ膜の成長に応じてN2ガス混合比を低下
させることで、第5図に示すごとく、なだらかなテーパ
を付与することができ、しかも配線抵抗の増加を抑える
ことができる。さらに、3段階、5段階と必要に応じて
N2混合比を変えたり、連続してN2混合比を変化させ
ることにより、ウェットエツチング加工によってなだら
かなテーパ形状を有する窒化モリブデン(MoXN)膜
4の積層膜からなるスパッタモリブデン膜の配線パタン
を形成することができる。その結果、上層配線の断線や
被覆した絶縁膜の耐圧低下等の多層配線の欠陥の発生を
効果的に防止することができる。
The results of this example show that by controlling the mixing ratio of N2 gas in the sputtering gas, it is possible to obtain a taper angle of the cross section of the batten by etching while suppressing an increase in wiring resistance. That is, according to the present invention, the N2 gas mixing ratio in the sputtering gas is increased at the beginning of sputtered film deposition, and the N2 gas mixing ratio is decreased as the sputtered film grows, as shown in FIG. , a gentle taper can be provided, and an increase in wiring resistance can be suppressed. Furthermore, by changing the N2 mixture ratio in 3rd and 5th stages as necessary, or by continuously changing the N2 mixture ratio, a molybdenum nitride (MoXN) film 4 having a gently tapered shape is laminated by wet etching. A wiring pattern of a sputtered molybdenum film can be formed. As a result, it is possible to effectively prevent the occurrence of defects in the multilayer wiring, such as disconnection of the upper layer wiring and reduction in withstand voltage of the covered insulating film.

〔発明の効果〕〔Effect of the invention〕

以上詳細に説明したごとく、本発明によるスパッタガス
に窒素ガスを混合してモリブデン膜をスパッタ法で堆積
し形成すれば、テーパ加工が難しかったモリブデンスパ
ッタ膜を、均質で緻密な膜組織とすることによってエツ
チング速度を低減し、バタン断面形状にテーパの付いた
加工を再現性よく得ることができる。
As explained in detail above, if a molybdenum film is deposited by sputtering by mixing nitrogen gas with the sputtering gas according to the present invention, the molybdenum sputtered film, which was difficult to taper, can be made into a homogeneous and dense film structure. By reducing the etching speed, it is possible to obtain a tapered cross-sectional shape of the batten with good reproducibility.

また、モリブデン堆積膜の成長に応して窒素ガスの混合
比を減少することで、バタン断面のテーパ加工の角度を
低減させることができ、上層の配線や絶縁膜の段差に起
因する欠陥の防止が可能となり、モリブデンスパッタ膜
がLS 1.薄膜デバイス等の多層配線での適用範囲を
拡大し得る効果がある。
In addition, by reducing the mixing ratio of nitrogen gas as the molybdenum deposited film grows, it is possible to reduce the taper angle of the cross section of the batten, thereby preventing defects caused by steps in the upper wiring or insulating film. The molybdenum sputtered film becomes LS1. This has the effect of expanding the scope of application in multilayer wiring such as thin film devices.

【図面の簡単な説明】[Brief explanation of drawings]

第1図は本発明のモリブデン膜の形成方法におけるスパ
ッタガス中の窒素ガス混合比とエツチング速度との関係
の一例を示すグラフ、第2図は従来のモリブデン膜にお
けるオーバハングを示す模式図、第3図は本発明の実施
例1における窒化モリブデン膜を用いた場合のテーパ形
状のバタン断面を示す模式図、第4図は本発明の実施例
2における窒化モリブデン膜とモリブデン膜との積層膜
のバタン断面を示す模式図、第5図は本発明の実施例2
において窒素ガス混合比を段階的に変えて形成した窒化
モリブデン膜のバタン断面形状を示す模式図である。 1・・・ガラス基板    2・・・ITO膜3・・・
モリブデン(MO)膜 4・・・窒化モリブデン(Mo、N)膜5・・・アルミ
ニウム(A Q )膜
FIG. 1 is a graph showing an example of the relationship between the nitrogen gas mixing ratio in the sputtering gas and the etching rate in the molybdenum film forming method of the present invention, FIG. 2 is a schematic diagram showing overhang in a conventional molybdenum film, and FIG. The figure is a schematic diagram showing the cross section of a tapered baton in the case of using a molybdenum nitride film in Example 1 of the present invention, and FIG. A schematic diagram showing a cross section, FIG. 5 is a second embodiment of the present invention
FIG. 3 is a schematic diagram showing the cross-sectional shape of a molybdenum nitride film formed by changing the nitrogen gas mixture ratio stepwise in FIG. 1...Glass substrate 2...ITO film 3...
Molybdenum (MO) film 4...Molybdenum nitride (Mo, N) film 5...Aluminum (AQ) film

Claims (1)

【特許請求の範囲】 1、スパッタ法によりモリブデン膜とアルミニウム膜を
重ねた積層膜を形成する方法において、上記モリブデン
膜の形成は、窒素ガスを混合したスパッタガスを用いて
堆積することを特徴とするモリブデン膜の形成方法。 2、請求の範囲第1項において、モリブデン膜の形成は
、スパッタガス中への窒素ガスの混合比を、モリブデン
膜の成長段階に応じて低減させながらモリブデン膜の堆
積を行うことを特徴とするモリブデン膜の形成方法。
[Claims] 1. A method for forming a laminated film in which a molybdenum film and an aluminum film are stacked by sputtering, characterized in that the formation of the molybdenum film is deposited using a sputtering gas mixed with nitrogen gas. A method for forming a molybdenum film. 2. In claim 1, the formation of the molybdenum film is characterized in that the molybdenum film is deposited while reducing the mixing ratio of nitrogen gas in the sputtering gas depending on the growth stage of the molybdenum film. Method of forming molybdenum film.
JP2124075A 1990-05-16 1990-05-16 Method for forming molybdenum film Expired - Lifetime JP3046829B2 (en)