JPH042B2 - - Google Patents
Info
- Publication number
- JPH042B2 JPH042B2 JP11640783A JP11640783A JPH042B2 JP H042 B2 JPH042 B2 JP H042B2 JP 11640783 A JP11640783 A JP 11640783A JP 11640783 A JP11640783 A JP 11640783A JP H042 B2 JPH042 B2 JP H042B2
- Authority
- JP
- Japan
- Prior art keywords
- wood
- hydrogen peroxide
- solution
- decolorizing
- cylinder
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired
Description
〔技術分野〕
この発明は木材の脱色法に関する。
〔背景技術〕
一般に、木材を脱色させる場合、木材を過酸化
水素液内に浸漬させることによつて行なわれる。
従来は、脱色液たる過酸化水素液内にアルカリを
混入させて過酸化水素液の自己分解による脱色作
用を促進させる方法が頻繁に行なわれていた。し
かし、この方法によれば、被処理物たる木材を脱
色液内に浸漬させる以前に、過酸化水素液の自己
分解がいたずらに進行し、大変な無駄になつてい
た。また、木材の汚れが脱色液中に広がり、脱色
液が汚染されてしまうという欠点があつた。そこ
で、木材をアルカリ液で前処理した後、過酸化水
素液による脱色処理を行なうという方法が開発さ
れた。この方法によつて、過酸化水素がいたずら
に分解されることがなくなつた。しかし、木材の
処理工程が増えたため、それだけ時間がかかつて
しまうという欠点が生じてしまつた。また、この
方法によつても、木材の汚れは脱色液中に持ち込
まれるため、依然として脱色液の汚染を抑制する
という課題は克服されなかつた。
〔発明の目的〕
そこで、この発明は、脱色液の汚染が抑制さ
れ、脱色が効果的かつ短時間に行なわれる木材の
脱色法を提供することを目的とする。
〔発明の開示〕
発明者らは以上の目的を達成するため鋭意検討
を重ね、この発明を完成した。
この発明は、木材の小片にまずアルカリ液を浸
透させ、つぎに過酸化水素液を浸透させて脱色を
行なう木材の脱色法であつて、木材の小片をアリ
カリ液に浸漬した状態で圧縮したのち、圧縮状態
のままで過酸化水素液中に移して上記圧縮の解放
を行なうようにすることを特徴とする木材の脱色
法をその要旨とする。以下、これを、その実施例
をあらわす図面に基づいて詳しく説明する。
第1図ないし第6図はこの発明にかかる木材の
脱色法の一実施例を説明する図面である。第1図
にみるように、多くの孔2…を有するシリンダ1
内に木材の小片4を充填する。充填後のシリンダ
1はピストン3を挿入しこれで蓋をする。そのよ
うなシリンダ1を、第2図にみるように、アルカ
リ液5内に浸漬する。つづいて、アルカリ液5内
でピストン3を押してシリンダ1内を圧縮する。
圧縮することによつて、木材の小片4…にアルカ
リ液5を充分に浸透させる。そして、第3図にみ
るように、さらに圧縮を行ない、木材の小片4…
に付着していた汚れをシリンダの孔2…からシリ
ンダ1外へと送り出すのである。なお、圧縮は1
度だけでなく繰り返し何度も行なつても構わな
い。つぎにピストンを押圧した状態のままシリン
ダをアルカリ液内から取り出し、第4図にみるよ
うに、そのまま過酸化水素液6内に浸漬する。つ
づいて、第5図にみるように、過酸化水素液6内
でピストン3を引き上げシリンダ1の圧縮を解放
する。圧縮解放とともにシリンダの孔2…からシ
リンダ1内に過酸化水素液6が入り込む。過酸化
水素液6は圧縮によつて減圧状態にある木材の小
片4…の内部に速やかに浸透し、既に浸透してい
たアルカリと接することによつて脱色作用が促進
されるのである。なお、圧縮解放は繰り返し何度
も行なわれても構わない。つづいて、過酸化水素
液内からシリンダを取り出し、第6図にみるよう
に、木材の小片4…の入つたシリンダ1にスチー
ム7による加熱処理を行なう。この加熱処理を行
なうことによつて脱色にかかる時間を短縮するこ
とができる。このようにして、木材の脱色を行な
うのである。
この発明にかかる木材の脱色法において被処理
物となる木材の小片は長さ2cm以内のものが好ま
しいがこれに限られるものではない。
アルカリ液として使用されるものは、NaOH
あるいはKOHの水溶液やそれら水溶液にケイ酸
ソーダまたはリン酸塩が混入されているものが好
ましい。
脱色液たる過酸化水素液は、20重量%(以下
「%」と略す)以上の過酸化水素水溶液であるこ
とが好ましい。
木材の小片を圧縮する方法は、実施例において
はシリンダが使用されていたが、これに限られる
ものではない。なお、圧縮時の圧力は、2Kg/cm2
以上であることが好ましい。
加熱処理の方法は、実施例においては、スチー
ムを当てる方法が用いられていたが、これ以外の
方法であつても構わない。加熱処理は、60℃以上
の温度で30分間以上行なうことが好ましい。
つぎに、この発明にかかる木材の脱色法による
実施例と従来の木材の脱色法による比較例とを挙
げ、その結果を表に示した。
〔実施例〕
アガチスのシユレツダーによる粉砕木片を、
NaOH 2%、水ガラス(3号)6%のアルカリ
溶液に浸漬し、アルカリ溶液内で木片に8Kg/cm2
の圧力をかけた。圧力をかけた状態の木片をアル
カリ溶液内から取り出し、そのままの状態で過酸
化水素の35%水溶液内に浸漬した。つづいて、過
酸化水素水溶液内で木片の圧力を解放した。その
後、木片を液内から取り出し、100℃のスチーム
で1時間加熱した。アルカリ溶液および過酸化水
素水溶液の浴比は30±10であつた。
〔比較例〕
アガチスのシユレツダーによる粉砕木片を、
NaOH 2%、水ガラス(3号)6%、過酸化水
素35%の60℃脱色液内に脱色度が上がらなくなる
まで浸漬した。浴比30±10であつた。
〔結果〕
[Technical Field] This invention relates to a method for decolorizing wood. [Background Art] Generally, when wood is decolored, the wood is immersed in a hydrogen peroxide solution.
Conventionally, a method has frequently been used in which an alkali is mixed into a hydrogen peroxide solution, which is a decolorizing solution, to promote the decolorizing action by self-decomposition of the hydrogen peroxide solution. However, according to this method, self-decomposition of the hydrogen peroxide solution progresses unnecessarily before the wood to be treated is immersed in the decolorizing solution, resulting in a great deal of waste. Another drawback was that the stains on the wood spread into the decolorizing solution, contaminating the decolorizing solution. Therefore, a method was developed in which wood is pretreated with an alkaline solution and then decolorized with a hydrogen peroxide solution. This method prevented unnecessary decomposition of hydrogen peroxide. However, because the number of wood processing steps increased, the disadvantage was that it took more time. Furthermore, even with this method, the stains on the wood are carried into the decolorizing solution, so the problem of suppressing contamination of the decolorizing solution has not yet been overcome. [Object of the Invention] Therefore, an object of the present invention is to provide a method for decolorizing wood in which contamination of the decolorizing solution is suppressed and decolorization is carried out effectively and in a short time. [Disclosure of the Invention] In order to achieve the above object, the inventors have made extensive studies and have completed this invention. This invention is a method of decolorizing wood by first impregnating small pieces of wood with an alkaline solution and then impregnating a hydrogen peroxide solution. The gist is a method for decolorizing wood, which is characterized by transferring the wood in a compressed state into a hydrogen peroxide solution to release the compression. Hereinafter, this will be explained in detail based on drawings showing examples thereof. FIGS. 1 to 6 are drawings illustrating an embodiment of the method for decolorizing wood according to the present invention. As shown in Fig. 1, a cylinder 1 with many holes 2...
Fill the inside with small pieces of wood 4. After filling the cylinder 1, a piston 3 is inserted and the cylinder 1 is covered. Such a cylinder 1 is immersed in an alkaline solution 5, as shown in FIG. Next, the piston 3 is pushed in the alkaline liquid 5 to compress the inside of the cylinder 1.
By compressing, the alkaline solution 5 is sufficiently penetrated into the small pieces of wood 4. Then, as shown in Figure 3, further compression is performed, and the small piece of wood 4...
The dirt adhering to the cylinder is sent out from the cylinder 1 through the cylinder hole 2. Note that the compression is 1
You can do it not only once, but also over and over again. Next, the cylinder is taken out of the alkaline solution while the piston is still being pressed, and is immersed in the hydrogen peroxide solution 6 as is, as shown in FIG. Subsequently, as shown in FIG. 5, the piston 3 is pulled up within the hydrogen peroxide solution 6 to release the compression of the cylinder 1. As compression is released, hydrogen peroxide liquid 6 enters into cylinder 1 from holes 2 of the cylinder. The hydrogen peroxide solution 6 quickly penetrates into the interior of the small piece of wood 4 under reduced pressure due to compression, and the decolorizing action is promoted by contacting with the alkali that has already penetrated. Note that the compression release may be repeated many times. Subsequently, the cylinder is taken out from the hydrogen peroxide solution, and as shown in FIG. 6, the cylinder 1 containing the small pieces of wood 4 is subjected to a heat treatment using steam 7. By performing this heat treatment, the time required for decolorization can be shortened. This is how the wood is bleached. In the method for decolorizing wood according to the present invention, the wood pieces to be treated preferably have a length of less than 2 cm, but are not limited thereto. What is used as alkaline solution is NaOH
Alternatively, an aqueous solution of KOH or an aqueous solution containing sodium silicate or phosphate is preferable. The hydrogen peroxide solution serving as the decolorizing solution is preferably an aqueous hydrogen peroxide solution containing 20% by weight (hereinafter abbreviated as "%") or more. Although a cylinder was used in the embodiment as a method for compressing small pieces of wood, the method is not limited to this. The pressure during compression is 2Kg/cm 2
It is preferable that it is above. In the example, a method of applying steam was used as the heat treatment method, but other methods may be used. The heat treatment is preferably performed at a temperature of 60° C. or higher for 30 minutes or longer. Next, examples using the wood bleaching method according to the present invention and comparative examples using the conventional wood bleaching method are listed, and the results are shown in the table. [Example] Pulverized wood chips using Agatis shredder,
Immerse in an alkaline solution of 2% NaOH and 6% water glass (No. 3), and apply 8 kg/cm 2 to a piece of wood in the alkaline solution.
pressure was applied. The piece of wood under pressure was taken out of the alkaline solution and immersed in a 35% aqueous solution of hydrogen peroxide. Next, the pressure on the wood pieces was released in a hydrogen peroxide solution. Thereafter, the wood pieces were taken out of the liquid and heated with steam at 100°C for 1 hour. The bath ratio of the alkaline solution and hydrogen peroxide aqueous solution was 30±10. [Comparative example] Pulverized wood chips using Agatis shredder,
It was immersed in a 60°C decolorizing solution containing 2% NaOH, 6% water glass (No. 3), and 35% hydrogen peroxide until the degree of decolorization no longer increased. The bath ratio was 30±10. 〔result〕
以上のように、この発明にかかる木材の脱色法
は、木材の小片にまずアルカリ液を浸透させ、つ
ぎに過酸化水素液を浸透させて脱色を行なう木材
の脱色法であつて、木材の小片をアルカリ液に浸
漬した状態で圧縮したのち、圧縮状態のままで過
酸化水素液中に移して上記圧縮の解放を行なうよ
うにすることを特徴としているので、過酸化水素
の余計な自己分解がなくなり、木材の汚れが圧縮
によつてアルカリ液中に送り出されるため、過酸
化水素液の汚染度が微少になり、圧縮と圧縮解放
によつてアルカリ液と過酸化水素液の木材への浸
透が促進するため、脱色にかかる時間が大幅に短
縮されるようになるという効果がもたらされるの
である。
As described above, the method for decolorizing wood according to the present invention is a method for decolorizing wood by first impregnating small pieces of wood with an alkaline solution and then impregnating a hydrogen peroxide solution. This method is characterized in that it is compressed while immersed in an alkaline solution, and then transferred to a hydrogen peroxide solution in the compressed state to release the compression, thereby eliminating unnecessary self-decomposition of hydrogen peroxide. Since the stains on the wood are sent out into the alkaline solution through compression, the degree of contamination from the hydrogen peroxide solution is minimal, and the compression and release of the compression prevent the penetration of the alkali solution and hydrogen peroxide solution into the wood. This has the effect of significantly shortening the time required for decolorization.
第1図ないし第6図はこの発明にかかる木材の
脱色法の一実施例について説明する断面図であ
る。
1……シリンダ、4……木材の小片、5……ア
ルカリ液、6……過酸化水素液、7……スチー
ム。
1 to 6 are cross-sectional views illustrating an embodiment of the method for decolorizing wood according to the present invention. 1... Cylinder, 4... Small piece of wood, 5... Alkaline solution, 6... Hydrogen peroxide solution, 7... Steam.
Claims (1)
ぎに過酸化水素液を浸透させて脱色を行なう木材
の脱色法であつて、木材の小片をアルカリ液に浸
漬した状態で圧縮したのち、圧縮状態のままで過
酸化水素液中に移して上記圧縮の解放を行なうよ
うにすることを特徴とする木材の脱色法。 2 過酸化水素液内から取り出した木材の小片に
対して加熱処理を行なう特許請求の範囲第1項記
載の木材の脱色法。[Scope of Claims] 1. A method for decolorizing wood by first impregnating a small piece of wood with an alkaline solution and then impregnating a hydrogen peroxide solution. A method for decolorizing wood, which comprises compressing the wood and then transferring the compressed state into a hydrogen peroxide solution to release the compression. 2. A method for decolorizing wood according to claim 1, wherein a small piece of wood taken out from a hydrogen peroxide solution is heat-treated.