JPH044121A - Transparent in-mold label - Google Patents

Transparent in-mold label

Info

Publication number
JPH044121A
JPH044121A JP2104107A JP10410790A JPH044121A JP H044121 A JPH044121 A JP H044121A JP 2104107 A JP2104107 A JP 2104107A JP 10410790 A JP10410790 A JP 10410790A JP H044121 A JPH044121 A JP H044121A
Authority
JP
Japan
Prior art keywords
label
layer
resin
thickness
mold
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP2104107A
Other languages
Japanese (ja)
Other versions
JP2848916B2 (en
Inventor
Masatsuki Yamanaka
昌月 山中
Yozo Oba
大庭 洋三
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Yupo Corp
Original Assignee
Yupo Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Yupo Corp filed Critical Yupo Corp
Priority to JP2104107A priority Critical patent/JP2848916B2/en
Publication of JPH044121A publication Critical patent/JPH044121A/en
Application granted granted Critical
Publication of JP2848916B2 publication Critical patent/JP2848916B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

PURPOSE:To obtain a label which does not peel off and has high adhesion, by a method wherein the present label is formed of a resin film which possesses a specific thickness, opaqueness and Clark degree in longitudinal and lateral directions. CONSTITUTION:A label 1 is formed of a resin film which has a thickness of 50-250 mum, opaqueness of 10% or lower and clark degree in longitudinal and lateral directions is 2-15. The resin film is comprised of a base layer 1a holding less than 15-50% of a thickness of the whole of the label and having the tensile modulus of elasticity of 8000-40000kg/cm<2> and an elastic resin layer 1b holding 50-80% of a thickness of the whole of the label laminated at least to one side of the base layer and having the tensile modulus of elasticity of 2000-6000 kg/cm<2>. Furthermore, the label 1 is provided with an adhesive layer 1d formed of resin holding 0.1-5% of a thickness of the whole of the label laminated to the surface opposite to the base layer of the elastic resin layer and having the melting point lower than the melting point of the resin forming the base layer by at least 10 deg.C.

Description

【発明の詳細な説明】 〔発明の背景〕 〈産業上の利用分野〉 本発明は、ブリスターの発生を防止した透明なインモー
ルド用ラベルに関する。
DETAILED DESCRIPTION OF THE INVENTION [Background of the Invention] <Industrial Application Field> The present invention relates to a transparent in-mold label that prevents blistering.

〈従来の技術〉 従来、透明のラベルが貼着した合成樹脂成形物を一体成
形により製造するには、結晶性ポリプロピレンの無延伸
の押出フィルムやキャスト法により成形された結晶性ポ
リプロピレンフィルムなどを基材層として、該基材層に
低密度ポリエチレン、エチレン・酢酸ビニル共重合体な
どの感熱接着樹脂層を直接押出ラミネートしたり、ポリ
酢酸ビニルやエチレン拳酢酸ビニル共重合体のような低
融点樹脂を溶剤に溶解させた溶液をグラビアコーターな
どでコーティングし乾燥して得られた透明なラベルを、
金型の内壁に予めインサートした後、該金型内にポリプ
ロピレンやポリエチレン樹脂などの成形用樹脂を直接供
給し、射出成形や中空成形成いは、型内ビーズ発泡成形
するなどの方法により行なわれていた。また、ポリプロ
ピレンやポリエチレンのシートにラベルを貼付する場合
も該シートを加熱し差圧に依って成形する差圧成形方法
(真空成形、圧空成形)もほぼ同様の方法により行なわ
れていた。
<Conventional technology> Conventionally, in order to manufacture a synthetic resin molded article with a transparent label attached by integral molding, a method using a base material such as an unstretched extruded film of crystalline polypropylene or a crystalline polypropylene film molded by a casting method has been used. As a material layer, a heat-sensitive adhesive resin layer such as low-density polyethylene or ethylene-vinyl acetate copolymer is directly extruded laminated to the base material layer, or a low-melting point resin such as polyvinyl acetate or ethylene-vinyl acetate copolymer is used. A transparent label obtained by coating a solution of dissolved in a solvent with a gravure coater etc. and drying it.
After inserting into the inner wall of a mold in advance, a molding resin such as polypropylene or polyethylene resin is directly supplied into the mold, and injection molding, hollow molding, or in-mold bead foam molding is performed. was. Furthermore, when attaching labels to sheets of polypropylene or polyethylene, substantially the same method has been used for differential pressure forming (vacuum forming, pressure forming) in which the sheet is heated and formed by differential pressure.

〈発明が解決しようとする課題〉 このような結晶性ポリプロピレンの押出フィルムやキャ
スト法によって得られた結晶性ポリプロピレンフィルム
を基材層とし、接着層としてエチレン系樹脂フィルムを
積層した透明のラベルを用いて、ポリプロピレンの中空
容器を加飾しようとすると、ポリプロピレンのパリソン
温度を230℃以上とし、かつ金型の冷却水温度を10
℃以上にしないと良好な製品を得ることができなかった
。
<Problem to be solved by the invention> A transparent label is used in which a base layer is such an extruded crystalline polypropylene film or a crystalline polypropylene film obtained by a casting method, and an ethylene resin film is laminated as an adhesive layer. When trying to decorate a polypropylene hollow container, the polypropylene parison temperature should be set to 230°C or higher, and the mold cooling water temperature should be set to 10°C.
A good product could not be obtained unless the temperature was above ℃.

また、このようなラベルはポリエチレン中空容器につい
てもポリプロピレンの中空容器と同様のパリソン温度と
金型冷却水の温度条件が不可欠であった。
In addition, for such a label, it is essential that the polyethylene hollow container has the same parison temperature and mold cooling water temperature conditions as the polypropylene hollow container.

一般にポリエチレン(融点119〜135℃)容器の中
空成形の高速化条件は、生産コストを考え合わせると、
パリソン温度を低くし、冷却時間を短かくすることが望
ましい。
In general, the conditions for increasing the speed of blow molding of polyethylene (melting point 119-135°C) containers are as follows, considering production costs:
It is desirable to lower the parison temperature and shorten the cooling time.

しかしなから、このような高速化条件を満たすことので
きる180〜210℃位のパリソン温度では、上記ポリ
プロピレンの2軸延伸フイルムやキャストフィルムより
なるラベルを用いたときに、ラベルと中空容器の接着強
度が低く、実用的なものか得られなかった。
However, at parison temperatures of about 180 to 210°C, which can satisfy such high-speed conditions, when labels made of the above-mentioned polypropylene biaxially stretched film or cast film are used, the adhesion between the label and the hollow container is difficult. The strength was low and it was not practical.

〔発明の概要〕[Summary of the invention]

く要 旨〉 そこで、本発明者は上記課題に鑑みて、鋭意研究を重ね
た結果、プロピレン単独重合体のキャストフィルムや二
軸延伸された結晶性ポリプロピレンフィルムを素材とす
るラベルの引張弾性率(ASTM  D−638)が約
8,500〜30、 000kg/cdで、クラーク剛
度が20〜40と高いため、溶融パリソンが膨張してラ
ベルと接着する際、パリソンの表面が曲面であるため、
ラベルにかかるパリソンの圧力か場所によって相違し、
部分的に強い接着部分と弱い接着部分とが存在し、かつ
、パリソンより形成された容器が冷却されたときに、結
晶性のポリプロピレンや結晶性のポリエチレンは寸法収
縮率が1,5〜3%と大きいことから、この収縮応力に
よって弱い接着部分に剥離が生じて、ブリスター発生を
起す原因となっていることが判明した。
Summary In view of the above problems, the present inventors have conducted intensive research and have determined the tensile modulus ( ASTM D-638) is approximately 8,500 to 30,000 kg/cd, and Clark stiffness is high at 20 to 40, so when the molten parison expands and adheres to the label, the surface of the parison is curved.
The pressure of the parison on the label varies depending on the location.
Crystalline polypropylene and crystalline polyethylene have a dimensional shrinkage rate of 1.5 to 3% when the container formed from the parison is cooled, and there are strong and weak adhesive areas in some parts. It was found that this shrinkage stress causes peeling in weakly bonded areas, causing blistering.

しかし、ラベルの引張弾性率やクラーク剛度を下げるに
は、発泡したラベルや、フィラーを配合して二軸延伸し
て得たフィルム内部に微細なボイドを多数有する合成紙
(特開昭58−69015号公報およびヨーロッパ公開
特許第254923号明細書参照)を用いれば、内部に
微細な空隙を多数含んでいるためにラベル内に延伸フィ
ルムを含んでいてもラベル自体に適度の圧縮性か杓−り
、又、金型内壁に装着された時に金型の表面温度かラベ
ル表面へ熱伝導され難く、ラベルの表面温度が低下する
ことを防いてラベルの変形やブリスタの発生を防止する
ことかできるか、これらのラベルは不透明のものであり
、透明なラベルとはならない。
However, in order to lower the tensile modulus and Clark stiffness of labels, foamed labels or synthetic paper (Japanese Patent Laid-Open No. 58-69015 Publication No. 254,923 (see European Patent Publication No. 254,923), even if the label contains a stretched film, the label itself has an appropriate degree of compressibility or ladle because it contains many fine voids inside. Also, when attached to the inner wall of the mold, the surface temperature of the mold is difficult to conduct heat to the label surface, and is it possible to prevent the label surface temperature from decreasing and prevent the deformation of the label and the generation of blisters? , these labels are opaque, not transparent labels.

また、透明ラベルにおいては、光沢の向上、印刷の保護
の理由から容器と接着されるラベルの接着面に印刷が施
こされることが多いので、不透明ラベルを用いたときは
かかる印刷が読みとれないなどの欠点を有していた。
In addition, for transparent labels, printing is often applied to the adhesive side of the label that is attached to the container to improve gloss and protect the printing, so such printing cannot be read when using opaque labels. It had drawbacks such as.

一方、従来の結晶性ポリプロピレン製の不透明度が10
%以下の透明ラベルは前記合成紙のような微細な空隙が
無いためにラベル自体のクラーク剛度が20〜40と硬
く、また熱伝導も大きいのでラベル表面が高温や低温に
なり易く、溶融樹脂によるラベル表面の接着層の樹脂を
短時間で溶融化させて貼着させるための条件の幅が狭い
。
On the other hand, the opacity of conventional crystalline polypropylene is 10
% or less transparent labels do not have minute voids like the synthetic paper mentioned above, so the label itself has a hard Clark stiffness of 20 to 40, and also has high heat conduction, so the label surface easily becomes hot or cold. The range of conditions for melting and sticking the adhesive layer resin on the label surface in a short time is narrow.

そこで、本発明者は更に研究を重ねた結果、該透明な基
材フィルム層と接着層との間に、引張弾性率が2,00
0〜6,000の弾性樹脂層を設けることによりラベル
全体のクラーク剛度を下げて、溶融パリソンの熱膨張や
容器の寸法収縮を該弾性樹脂層によって吸収すれば、ラ
ベルの変形やブリスターの発生が生じないラベル付きの
成形物が得られるとの知見を得て本発明を完成するに至
った。
Therefore, as a result of further research, the present inventor found that the tensile modulus between the transparent base film layer and the adhesive layer was 2,000.
By providing an elastic resin layer of 0 to 6,000, the Clark stiffness of the entire label can be lowered, and if the thermal expansion of the molten parison and the dimensional contraction of the container are absorbed by the elastic resin layer, deformation of the label and generation of blisters can be prevented. The present invention was completed based on the knowledge that a molded product with a label that does not occur can be obtained.

すなわち、本発明の透明なインモールド用ラベルは、厚
さが50〜250μtmで、不透明度か10%以下、縦
方向及び横方向のクラーク剛度が2〜15の樹脂フィル
ムより形成されていること、を特徴とするものである。
That is, the transparent in-mold label of the present invention is formed from a resin film having a thickness of 50 to 250 μtm, an opacity of 10% or less, and a Clark stiffness in the longitudinal and lateral directions of 2 to 15. It is characterized by:

く効 果〉 本発明の透明なインモールド用ラベルは、X材層と接着
層の間に弾性樹脂層を設けてラベル全体のクラーク剛度
を低下させて形成したことから、溶融パリソンを成形加
工してラベルを貼着する際の熱膨張や容器の寸法収縮を
生じても、弾性樹脂層が貼着した状態で容易に変形する
ことができるので、ラベルの剥離が起らず、また接着強
度の強いラベルか得られる。
Effect> The transparent in-mold label of the present invention is formed by providing an elastic resin layer between the X material layer and the adhesive layer to reduce the Clark stiffness of the entire label. Even if there is thermal expansion or dimensional contraction of the container when attaching the label, the elastic resin layer can be easily deformed while attached, so the label will not peel off and the adhesive strength will be reduced. You will get a strong label.

従ってポリプロピレンやポリエチレンの成形加工条件に
おいても樹脂温度の設定か低温側に設定したり、又金型
の冷却温度を下げて成形サイクルを短くすることができ
るので、生産性が大巾に向上し、かつ、得られる成形物
のラベルにブリスターの発生が少ない外観に優れ、しか
もラベルと容器との密着性の優れた、ラベルの貼着され
た一体成形品を製造することが出来る。
Therefore, even in the molding processing conditions for polypropylene and polyethylene, it is possible to set the resin temperature to a lower temperature side, or to lower the cooling temperature of the mold to shorten the molding cycle, greatly improving productivity. Moreover, it is possible to produce an integrally molded product with a label attached thereto, which has an excellent appearance with little blister generation on the label of the resulting molded product, and has excellent adhesion between the label and the container.

〈発明の具体的説明〉 [1]インモールド用ラベル (1)構造 本発明の透明なインモールド用ラベルは、縦方向及び横
方向のクラーク剛度が2〜15の厚さ50〜250μt
mの樹脂フィルムであれば、単層であっても、或いは2
層以上の構造のものであってもよいか、好適には二軸延
伸された基材層と、その少なくとも片面に積層された弾
性樹脂層と、該弾性樹脂層の基材層と反対側の面に形成
された感熱接着層とから基本的に構成される3層構造以
上のものである。
<Specific description of the invention> [1] In-mold label (1) Structure The transparent in-mold label of the present invention has a Clark stiffness of 2 to 15 in the longitudinal and lateral directions and a thickness of 50 to 250 μt.
m resin film, even if it is a single layer or two layers.
It may have a structure of more than one layer, or preferably a biaxially stretched base material layer, an elastic resin layer laminated on at least one side of the biaxially stretched base layer, and an elastic resin layer on the opposite side of the base material layer. It has a three-layer structure or more basically consisting of a heat-sensitive adhesive layer formed on the surface.

以下にその好適な場合の構造について具体的に記載する
。
The preferred structure will be specifically described below.

(a)基材層 基材層に用いられる樹脂フィルムとしては、ポリプロピ
レン、高密度ポリエチレン、低密度ポリエチレン、ポリ
アミド樹脂、ポリエステル樹脂などの成形体用樹脂を一
軸延伸又は二軸延伸して得られた延伸フィルムである。
(a) Base material layer The resin film used for the base material layer is obtained by uniaxially or biaxially stretching resin for moldings such as polypropylene, high density polyethylene, low density polyethylene, polyamide resin, polyester resin, etc. It is a stretched film.

このような基材層の厚みは、ラベル全体の厚みの一般に
50%未満、好ましくは15〜48%の範囲内で用いら
れる。
The thickness of such a base layer is generally less than 50% of the total thickness of the label, preferably within the range of 15 to 48%.

この基材層の厚みがラベル全体の50%を超えるとクラ
ーク剛度が15を超えるようになるので、ブリスター適
性や接着強度が著しく低下して来る。
If the thickness of this base layer exceeds 50% of the entire label, the Clark stiffness will exceed 15, resulting in a significant decrease in blister suitability and adhesive strength.

また、15%未満の場合はラベルの引張強度が低下して
印刷が困難となったり、吸引パッドで金型内に自動的に
供給することが困難となる。
Furthermore, if it is less than 15%, the tensile strength of the label decreases, making it difficult to print or automatically feeding into the mold with a suction pad.

(b)弾性樹脂層 前記基材層のみで構成されるラベルはクラーク剛度が2
0を超えるものであることから、その−部に弾性樹脂層
を設けてラベル全体のクラーク剛度を低下させることが
重要である。
(b) Elastic resin layer The label composed only of the base material layer has a Clark stiffness of 2.
Since the stiffness exceeds 0, it is important to provide an elastic resin layer in the negative part to reduce the Clark stiffness of the entire label.

このようなラベル全体のクラーク剛度を低下させる弾性
樹脂として用いられる素材としては、引張弾性率が2.
 000〜6. 000kg/cd、好ましくは2.5
00〜4,800kg/cm2のものである。
The material used as the elastic resin that reduces the Clark stiffness of the entire label has a tensile modulus of 2.
000~6. 000kg/cd, preferably 2.5
00 to 4,800 kg/cm2.

このような引張弾性率の値を示す樹脂としては、例えば
、プロピレンか80〜97重量%、エチレンが2〜20
重量%、ブテン−1が1〜12重量%を2P!又は3種
含有するランダム又はブロック状の共重合体もしくはそ
れらの混合物を挙げることができ、具体的には、プロピ
レンを80〜95重量%、エチレンを20〜5重量%含
有するプロピレン・エチレン共重合体、プロピレンを8
0〜95重量%、ブテン−1を20〜5重量%含有する
プロピレン・ブテン−1共重合体、プロピレンを80〜
95重量%、エチレンを0.5〜12重量%、ブテン−
1を2〜10重量%含有するプロピレン・エチレン・ブ
テン−1共重合体などまたはその混合物である。
Examples of resins exhibiting such tensile modulus values include propylene of 80 to 97% by weight and ethylene of 2 to 20% by weight.
% by weight, butene-1 is 1 to 12% by weight 2P! Or a random or block copolymer containing three types, or a mixture thereof. Specifically, a propylene/ethylene copolymer containing 80 to 95% by weight of propylene and 20 to 5% by weight of ethylene. Combine, propylene 8
Propylene-butene-1 copolymer containing 0 to 95% by weight and 20 to 5% by weight of butene-1, 80 to 95% by weight of propylene.
95% by weight, 0.5-12% by weight of ethylene, butene-
It is a propylene-ethylene-butene-1 copolymer containing 2 to 10% by weight of 1, or a mixture thereof.

また、これら共重合体成分を構成するモノマーとして、
上記プロピレン・エチレン、ブテン−1の他に更に少j
l(0,5%〜5重量%)のヘキセン−1、ペンテン−
1,4−メチルペンテン−1などのα−オレフィンより
選ばれた一種又は二種以上を含んだものとのランダムも
しくはブロック共重合体が使用できる。
In addition, as monomers constituting these copolymer components,
In addition to the above propylene/ethylene and butene-1, even less
l (0.5% to 5% by weight) of hexene-1, pentene-1
Random or block copolymers containing one or more α-olefins such as 1,4-methylpentene-1 can be used.

これら弾性樹脂層の厚みは一般にラベル肉厚の50〜8
5%である。また、不透明度(JIS−P8138)が
10%以下のものが好ましい。
The thickness of these elastic resin layers is generally 50 to 8 times the thickness of the label.
It is 5%. Further, it is preferable that the opacity (JIS-P8138) is 10% or less.

さらに、これら弾性樹脂層は積層されたものより構成さ
れていても良い。
Furthermore, these elastic resin layers may be constructed by laminating them.

(c)接着層 前記弾性樹脂層を介して基材層に積層される接着層とし
ては、接着される成形体材料の融点よりも10℃以上、
好ましくは15〜100℃低い、融点が70〜155℃
、好ましくは80〜130℃の熱可塑性樹脂か利用され
る。
(c) Adhesive layer The adhesive layer laminated to the base material layer via the elastic resin layer is 10° C. or higher than the melting point of the molded material to be bonded;
Preferably 15-100°C lower, melting point 70-155°C
A thermoplastic resin having a temperature of preferably 80 to 130° C. is used.

例えば、接着される成形体材料かポリプロピレン系樹脂
である場合には、低密度ポリエチレン、エチレン・酢酸
ビニル共重合体、エチレン・アクリル酸共重合体、もし
くはその金属塩などのエチレン系樹脂が用いられる。
For example, if the molded material to be bonded is a polypropylene resin, an ethylene resin such as low density polyethylene, ethylene/vinyl acetate copolymer, ethylene/acrylic acid copolymer, or a metal salt thereof is used. .

また、接着される成形体材料かポリエチレン系樹脂であ
る場合には、該ポリエチレン系樹脂より融点の低いエチ
レン・酢酸ビニル共重合体、エチレン・アクリル酸共重
合体、もしくはその金属塩などが用いられる。
In addition, if the molding material to be bonded is a polyethylene resin, an ethylene/vinyl acetate copolymer, an ethylene/acrylic acid copolymer, or a metal salt thereof, which has a lower melting point than the polyethylene resin, is used. .

これらの感熱樹脂接着層は弾性樹脂層上に押出ラミネー
トして形成したり、それら接着用樹脂を溶剤に溶解した
液をグラビアコーターによりコーティングし、乾燥して
成形させる。押出ラミネートの場合は弾性樹脂層を形成
する際に別々の押出機を用いてダイ内で接着層樹脂が外
側にくる様にラミネートして形成する方法と一般的な押
出ラミネート法によるラミネートの方法がある。いずれ
の押出ラミネートの場合も容器に貼着された場合に接着
強度の強いラベルを得ることができる。また、グラビア
コーターによるコーティング方式はグラビア印刷と同時
に接着層のコーティングも一挙にてき、また、薄肉とす
ることができるので経済的に有利なラベルを得ることが
できる。
These heat-sensitive resin adhesive layers are formed by extrusion lamination on the elastic resin layer, or are coated with a liquid obtained by dissolving these adhesive resins in a solvent using a gravure coater, and dried and molded. In the case of extrusion lamination, when forming the elastic resin layer, there are two methods: one is to use a separate extruder and laminate in a die so that the adhesive layer resin is on the outside, and the other is to use the general extrusion lamination method. be. Any extrusion laminate can provide a label with strong adhesive strength when applied to a container. Furthermore, in the coating method using a gravure coater, the adhesive layer can be coated at the same time as gravure printing, and the label can be made thinner, making it possible to obtain an economically advantageous label.

これら接着層はラベルと溶融した樹脂との間の空気の逃
げを良好にしてブリスターの発生を防止する為に、ラミ
ネートの際にはエンボス加工を施したり、グラビヤコー
ティングの際にはグラビヤのパターンが表面に残る様な
コーティング方法を施すことが望ましい。
These adhesive layers are embossed during lamination, and gravure patterns are applied during gravure coating to ensure good air escape between the label and the molten resin and prevent blistering. It is desirable to apply a coating method that leaves a residue on the surface.

また、このような接着層の厚みは一般的にはグラビアコ
ーティングの場合は0.05μ〜12.5μ、好ましく
は0. 5μ〜10μである。
Further, the thickness of such an adhesive layer is generally 0.05μ to 12.5μ in the case of gravure coating, preferably 0.05μ to 12.5μ. It is 5μ to 10μ.

また、押出ラミネートの場合は0. 5μ〜25μ、好
ましくは1〜20μ、なお、押出ラミネート品は延伸に
より、0.5μ〜10μの薄い接着層とすることができ
る。
In addition, in the case of extrusion laminate, 0. The adhesive layer has a thickness of 5μ to 25μ, preferably 1 to 20μ, and the extrusion laminate can be made into a thin adhesive layer of 0.5μ to 10μ by stretching.

(d)積層 前記基材層、弾性樹脂層および接着層は、接着層が弾性
樹脂層を介して基材層に積層することか重要である。
(d) Lamination Regarding the base material layer, elastic resin layer, and adhesive layer, it is important that the adhesive layer is laminated to the base material layer via the elastic resin layer.

積層は一般に押出ラミネート法、グラビアコーティング
法などの方法によって行なわれる。
Lamination is generally performed by a method such as an extrusion lamination method or a gravure coating method.

また、前記基材層の接着層か積層される側と反対の側に
は更に他の樹脂層を積層することもてきる。
Further, another resin layer may be further laminated on the side of the base material layer opposite to the side on which the adhesive layer is laminated.

(2)印刷 前記弾性樹脂層は接着層を設ける前に印刷を施してその
上に接着層を設ける方法や、該接着層と反対側の基材層
の表面に印刷を施す方法がある。
(2) Printing The elastic resin layer may be printed before the adhesive layer is provided, and an adhesive layer may be formed thereon, or the elastic resin layer may be printed on the surface of the base material layer on the opposite side to the adhesive layer.

また、この基材層の印刷層面には、予め印刷適性を向上
させる為にコロナ放電処理やポリエチレンイミンの様な
アンカーコーティング剤や帯電防止剤等を塗工しておく
ことが好ましい。
Further, it is preferable that the printing layer surface of this base material layer is previously subjected to corona discharge treatment or coated with an anchor coating agent such as polyethyleneimine, an antistatic agent, etc. in order to improve printing suitability.

印刷はグラビヤ印刷、オフセット印刷、フレキソ印刷、
スクリーン印刷などの印刷方法で接着層側に印刷したり
又はその反対側に印刷を施すことができる。
Printing includes gravure printing, offset printing, flexo printing,
Printing can be performed on the adhesive layer side or on the opposite side using a printing method such as screen printing.

本発明の詳細な説明ラベルの場合は成形物の色と同色の
色をラベル地として使用されて、弾性樹脂層の接着層が
積層される側に印刷されることが多く、このような印刷
は印刷面がラベルの内側になるために、商品となった時
に成形物どうしのこすれや成形物を入れる函等とのこす
れ等に依る印刷インキの脱落が起らないなどの利点があ
る。
Detailed explanation of the invention In the case of labels, the same color as the color of the molded product is used as the label material, and is often printed on the side of the elastic resin layer on which the adhesive layer is laminated. Since the printed surface is on the inside of the label, there are advantages such as the fact that when the product is made into a product, the printing ink does not fall off due to rubbing between the molded products or the box in which the molded products are placed.

(3)ラベル このようにして形成された透明なインモールド用ラベル
は不透明度(J I 5−P8138)が10%以下の
ものが好ましい。しかも縦方向及び横方向のクラーク剛
度が2〜15で、厚さが50〜250μtm1好ましく
は50〜150μtmであることから、該ラベルは成形
物が成形加工されて貼着された後の製品容器の収縮にも
ラベル自体が貼着された状態で容易に対応することがで
きるので、該ラベルと成形物表面において強固に接着さ
れて剥離が生じ難く、ラベルの変形やブリスターの発生
が生じない。
(3) Label The transparent in-mold label thus formed preferably has an opacity (J I 5-P8138) of 10% or less. Moreover, since the Clark stiffness in the longitudinal and lateral directions is 2 to 15, and the thickness is 50 to 250 μtm1, preferably 50 to 150 μtm, the label can be attached to the product container after the molded product has been formed and pasted. Since the label itself can easily cope with shrinkage while it is attached, the label and the surface of the molded product are firmly adhered to each other, making it difficult for peeling to occur, and preventing deformation of the label and generation of blisters.

前記クラーク剛度が2未満では印刷を行なうことが困難
であり、また、ラベルを金型の内壁にインサートするこ
とができない。また、クラーク剛度が15を超えるとブ
リスター適性や接着強度か低下する。
If the Clark stiffness is less than 2, it is difficult to print, and the label cannot be inserted into the inner wall of the mold. Furthermore, if the Clark stiffness exceeds 15, the blister suitability and adhesive strength will decrease.

また不透明度(J l5−P8138)が10%を超え
ると美麗な印刷を施しても不鮮明なものとなり、ラベル
の実用性を低下させる。
Furthermore, if the opacity (J 15-P8138) exceeds 10%, even beautiful printing becomes unclear, reducing the practicality of the label.

[11)貼着 本発明の透明インモールド用ラベルを一体成形して貼着
する際に用いられる成形法は、一般的に知られた中空成
形法や射出成形法、差圧成形法、型内ビーズ発泡成形法
、プレス成形法などによるものであり、公知の成形法と
何ら変わりな〈実施することができる。
[11) Adhesion Molding methods used when integrally molding and pasting the transparent in-mold label of the present invention include generally known blow molding methods, injection molding methods, differential pressure molding methods, and in-mold molding methods. It is based on a bead foam molding method, a press molding method, etc., and can be carried out in the same manner as known molding methods.

具体的には中空成形法の場合は予め前記ラベルの接着層
側を金型内壁面の内側に向けてインサートした後、該金
型内に押出機によって溶融混練させたポリプロピレン樹
脂あるいはポリエチレン樹脂などの成形用樹脂のパリソ
ンを180℃〜230℃の温度で垂下して、その一端を
型締めにより封止した後、該パリソンの内部に0.5〜
10kg/cdG、好ましくは2〜5kg/cシGの圧
縮ガスを導入することによりパリソンを膨張させる。
Specifically, in the case of the blow molding method, after inserting the label in advance with the adhesive layer side facing inside the inner wall surface of the mold, a polypropylene resin or polyethylene resin, etc., melt-kneaded by an extruder is inserted into the mold. A parison of molding resin is suspended at a temperature of 180°C to 230°C, and one end of the parison is sealed by mold clamping, and then 0.5 to
The parison is expanded by introducing compressed gas at 10 kg/cdG, preferably 2-5 kg/cdG.

これによってパリソンの外側の面を金型の内壁に押圧し
て、該パリソンの金型の形状に沿った形状に成形すると
共に、前記金型の内壁にインサートされたラベルの接着
層に溶融したパリソンを接着させて、ラベルの接着層の
樹脂を溶融してパリソンとラベルの接着層とを融着させ
た後、冷却して、金型を開き、ラベル付きの中空成形容
器を得る。
As a result, the outer surface of the parison is pressed against the inner wall of the mold, and the parison is molded into a shape that follows the shape of the mold, and the parison is fused to the adhesive layer of the label inserted into the inner wall of the mold. The resin of the adhesive layer of the label is melted to fuse the parison and the adhesive layer of the label, and then the parison is cooled and the mold is opened to obtain a hollow-molded container with a label.

〔実験例〕[Experiment example]

本発明の透明インモールド用ラベルについて、以下に実
施例および比較例を挙げて具体的に説明する。
The transparent in-mold label of the present invention will be specifically described below with reference to Examples and Comparative Examples.

実施例1 1〉積層配向フィルムの製造 メルトフローレート(MFR)4g/l 0分、エチレ
ン5重量96、プロピレン95重量9oのポリプロピレ
ン系ランダム共重合体を250℃に設定した押出機のダ
イより押し出し、ロール群の周速差を利用して縦延伸を
145℃で、縦延伸倍率を5倍にして延伸を行なった。
Example 1 1> Production of laminated oriented film Melt flow rate (MFR) 4 g/l 0 minutes, ethylene 5 weight 96, propylene 95 weight 9 o polypropylene random copolymer was extruded from the die of an extruder set at 250°C. Stretching was carried out at 145° C. and at a longitudinal stretching ratio of 5 times using the difference in circumferential speed between the roll groups.

一方、kiFR4g/10分、エチレン5重;%、プロ
ピレン95重量%のポリプロピレン系ランダム共重合体
を、250℃に設定した2台の押出機のダイより押し出
し、前記縦延伸フィルムの表裏面にラミネートし、−旦
、50℃まで冷却後、155℃まで加熱し、同温度でテ
ンターを用い、横方向に9倍延伸し162℃でアニーリ
ング処理し、再び30℃まで冷却し、耳部をスリットし
て三層構造の積層配向フィルムを得た。
On the other hand, a polypropylene random copolymer containing 4 g/10 min of kiFR, 5 wt.% ethylene, and 95 wt.% propylene was extruded through the dies of two extruders set at 250°C and laminated on the front and back surfaces of the longitudinally stretched film. Then, after cooling to 50°C, it was heated to 155°C, stretched 9 times in the transverse direction using a tenter at the same temperature, annealed at 162°C, cooled again to 30°C, and the edges were slit. A laminated oriented film with a three-layer structure was obtained.

2)印刷及び接着層(1d)の製造 上記三層構造の積層配向フィルム(1軸/2軸/1軸)
の両側にコロナ放電処理を施した後、アグリル系帯電防
止剤とポリエチレンイミンが配合された水溶液をO,1
g/rdの塗工量となる様に塗布した。この基材層(A
)の片面に容器の内容物、商品名、成分、製造元、販売
元等をグラビヤインキで印刷した後、この印刷面に、更
にグラビヤコーターによって塗工量か3g1rdとなる
様にエチレン・酢酸ビニール共重合体を主成分とする溶
剤型感熱接着剤(東洋モートン社製アトコート33P5
商品名)をグラビヤロールを用いて塗工し、乾燥して印
刷され、接着層を施したフィルムを得た。このフィルム
の物性を第1表に示す。
2) Printing and production of adhesive layer (1d) Laminated oriented film with the above three-layer structure (uniaxial/biaxial/uniaxial)
After applying corona discharge treatment to both sides of the
The coating was applied in a coating amount of g/rd. This base material layer (A
) After printing the contents of the container, product name, ingredients, manufacturer, distributor, etc. with gravure ink on one side of the paper, apply ethylene and vinyl acetate to the printed surface using a gravure coater to a coating amount of 3g1rd. Solvent-type heat-sensitive adhesive whose main component is a polymer (Atocoat 33P5 manufactured by Toyo Morton Co., Ltd.)
(trade name) using a gravure roll, dried and printed to obtain a film with an adhesive layer. The physical properties of this film are shown in Table 1.

3)ラベルの製造 前記フィルムを縦70關、横9011I11に断裁して
ラベルを製造した。
3) Manufacture of label The film was cut into 70 mm lengthwise and 9011 mm wide length to manufacture a label.

4)ラベル貼着中空容器の製造 前記ラベル1を第1図に示す中空成形容器製造用成形機
2の金型3内に、印刷層1c側を41℃に加熱された金
型3の内壁3aの真空減圧作用によりラベル1を金型内
壁3aに定着させた後、三菱油化■製ポリプロピレン「
三菱ノーブノンMA−6J(融点−164℃、MFR−
0,8)をダイ4より210℃の温度で、内径20關、
肉厚3 mmのパリソン5として押出し、このパリソン
5を金型3て挾みつけた後、ノズル6より圧力3 、 
5 kg / cdの圧縮空気をパリソン5内に供給し
て、ブロー成形すると共に、パリソン5の外面5aによ
り前記ラベル1を押圧してラベル1の接着層1d而を溶
融させてパリソン5にラベル1を融着させた後、金型3
を10℃に冷却して成形体を固化させ、型開きして、ラ
ベル1を貼着した胴直径が 60mm、高さが200m
mの中空容器(肉厚llll11)を得た。
4) Manufacture of label-attached hollow container The label 1 was placed in a mold 3 of a molding machine 2 for manufacturing a hollow molded container shown in FIG. After fixing the label 1 to the inner wall 3a of the mold by the vacuum decompression action of
Mitsubishi Norvenon MA-6J (melting point -164℃, MFR-
0,8) from die 4 at a temperature of 210℃, inner diameter 20mm,
After extruding it as a parison 5 with a wall thickness of 3 mm and sandwiching this parison 5 between the molds 3, a pressure of 3 mm is applied from the nozzle 6.
5 kg/cd of compressed air is supplied into the parison 5 for blow molding, and the outer surface 5a of the parison 5 presses the label 1 to melt the adhesive layer 1d of the label 1, thereby attaching the label 1 to the parison 5. After welding, mold 3
The molded body was cooled to 10°C to solidify, the mold was opened, and the body with label 1 attached had a diameter of 60 mm and a height of 200 m.
A hollow container (wall thickness 1111) was obtained.

また、同様の方法でパリソンの温度を230℃に変更し
て実施した。
Further, the same method was carried out with the temperature of the parison changed to 230°C.

さらに、三菱油化■製 高密度ポリエチレン(HDPE
)r三菱ポリエチJ(D  BZ−53AJを180℃
のパリソン温度で行なってラベル貼着中空容器を得た。
In addition, high-density polyethylene (HDPE) manufactured by Mitsubishi Yuka ■
) r Mitsubishi Polyethylene J (D BZ-53AJ at 180℃
The labeling process was carried out at a parison temperature of 100 mL to obtain a labeled hollow container.

得られたラベル貼着中空容器についてブリスターの発生
及びラベルの接着強度を検査した結果を第1表に示す。
Table 1 shows the results of testing the resulting labeled hollow containers for blister formation and label adhesive strength.

なお、これらの検査は次に示す方法により行なった。Note that these tests were conducted using the following method.

ブリスターの測定 容器1個につき、貼着されたラベルにブリスターの発生
か全くなかったものを5点、ラベル面積の10%以下で
ブリスターの発生のあったものを4点、10%以上、2
0%未満の面積でブリスターの発生があったものを3点
、20%以上、50%未満の面積でブリスターの発生の
あったものを2点、50%以上の面積の割合でブリスタ
ーの発生があったものを1点として容器の20個の総点
数で評価した。
For each blister measurement container, 5 points are given for those with blister formation or no blisters on the attached label, 4 points are given for those with blister formation on less than 10% of the label area, and 2 points are given for 10% or more of the label area.
3 points were given for cases where blisters occurred on less than 0% of the area, 2 points were given for cases where blisters were formed on 20% or more and less than 50% of the area, and 2 points were given for cases where blisters occurred on 50% or more of the area. The container was evaluated using a total score of 20, with each container being counted as 1 point.

ラベルと容器との間の帯青強度 ラベルの貼着された部分の容器を15mm1’llに切
り取り、引張試験機にてラベルの剥離強度を測定した。
Blue-tinged Strength Between the Label and the Container The portion of the container to which the label was attached was cut to 15 mm 1'll, and the peel strength of the label was measured using a tensile tester.

実施例2〜8及び比較例1〜4 第1表に示す基材層、表面層、裏面層の樹脂成分、延伸
軸数および肉厚に変更した以外は実施例1と同様の方法
で実施した。
Examples 2 to 8 and Comparative Examples 1 to 4 It was carried out in the same manner as in Example 1, except that the resin components, number of stretching axes, and wall thickness of the base layer, surface layer, and back layer shown in Table 1 were changed. .

その結果を第1表に示す。The results are shown in Table 1.

なお、裏面及び表面層のホモポリプロピレンの引張弾性
率は9. 000kg/cd、プロピレン(98%)・
エチレンランダム共重合体のそれは7.000kg/c
d、プロピレン(9596)・エチレンランダム共重合
体のそれは4,900kg/cd、プロピレン(95%
)・ブテン−1ランダム共重合体のそれは3. 500
kg/cd、プロピレン(85%)・エチレン(10%
)ブテン−1ランダム共重合体のそれは2,500kg
/cシてあった。
The tensile modulus of the homopolypropylene for the back and front layers is 9. 000kg/cd, propylene (98%)
That of ethylene random copolymer is 7.000 kg/c
d, that of propylene (9596)/ethylene random copolymer is 4,900 kg/cd, propylene (95%
)・butene-1 random copolymer is 3. 500
kg/cd, propylene (85%)/ethylene (10%
) Butene-1 random copolymer weighs 2,500 kg
/c was written.

実施例9 [)ラベル基材層(1a)の製造 メルトフローレート(MFR)4g/l 0分、エチレ
ン5重量%、プロピレン95重量%のポリプロピレン系
ランダム共重合体を250℃に設定した押出機のダイよ
り押し出し、縦延伸を145℃で、5倍に縦延伸を行な
って一軸延伸フィルムを得た。
Example 9 [) Production of label base material layer (1a) Melt flow rate (MFR) 4 g/l 0 minutes, polypropylene random copolymer containing 5% by weight of ethylene and 95% by weight of propylene in an extruder set at 250°C The film was extruded through a die and subjected to longitudinal stretching at 145°C to a factor of 5 to obtain a uniaxially stretched film.

2)ラベル弾性樹脂層(表面層(1b)裏面層一方、M
FR4g/10分、エチレン5重量%、プロピレン95
重量%のポリプロピレン系ランダム共重合体と、エチレ
ン80重量%、アクリル酸メチルエステル20重量%の
エチレン系ランダム共重合体を230℃に設定した別々
の2台の押出機のダイ内で積層し、エチレン系ランダム
共重合体が外側になるように前記l)の基材層に押出ラ
ミネートした。また前記基材層の反対面にはMFR4g
/10分、エチレン5重量%、プロピレン95重量%の
ポリプロピレン系ランダム共重合体を230℃に設定し
た押出機のダイより押し出し、基材層にラミネートし、
次いて、155℃の温度で9倍に横延伸を行なって四層
構造のフィルムを得た。
2) Label elastic resin layer (surface layer (1b), back layer, M
FR4g/10min, ethylene 5% by weight, propylene 95
A polypropylene random copolymer of % by weight and an ethylene random copolymer of 80% by weight of ethylene and 20% by weight of acrylic acid methyl ester were laminated in the dies of two separate extruders set at 230 ° C. The ethylene random copolymer was extrusion laminated onto the base material layer of 1) above so that it was on the outside. Also, on the opposite side of the base layer, MFR4g
/10 minutes, a polypropylene random copolymer containing 5% by weight of ethylene and 95% by weight of propylene was extruded through the die of an extruder set at 230°C, and laminated on the base material layer.
Next, the film was laterally stretched 9 times at a temperature of 155° C. to obtain a film having a four-layer structure.

3)印刷 上記四層構造の積層フィルムの裏面層(IC)面にコロ
ナ放電処理を施した後、アクリル系帯電防止剤とポリエ
チレンイミンとが配合された水溶液を0.1g/dの塗
工量となる様に塗布した。
3) Printing After corona discharge treatment is applied to the back layer (IC) surface of the four-layer laminated film described above, a coating amount of 0.1 g/d of an aqueous solution containing an acrylic antistatic agent and polyethyleneimine is applied. It was applied so that

この面に商品名、成分、製造元、販売元などをグラビア
インキで印刷した四層構造の積層フィルムを得た。この
フィルムの物性を第1表に示す。
A four-layer laminated film was obtained on which the product name, ingredients, manufacturer, distributor, etc. were printed with gravure ink. The physical properties of this film are shown in Table 1.

実施例10 ■)ラベル基材層(1a)の製造 メルトフローレート(VFR)4g/10分、エチレン
5重量%、プロピレン95重量%のポリプロピレン系ラ
ンダム共重合体を250℃に設定した押出機のダイより
押し出し、縦延伸を145℃で、縦方向に5倍延伸した
。
Example 10 ■) Production of label base material layer (1a) A polypropylene random copolymer with a melt flow rate (VFR) of 4 g/10 min, 5% by weight of ethylene, and 95% by weight of propylene was heated in an extruder set at 250°C. It was extruded from a die and stretched 5 times in the longitudinal direction at 145°C.

一方、MFR4g/10分、エチレン5重量%、プロピ
レン95重量96のポリプロピレン系ランダム共重合体
を250℃に設定した2台の押出機のダイより押し出し
、前記!)のフィルムの両面にラミネートし、次いで、
155℃の温度で横方向に9倍延伸を行なって162℃
でアニーリング処理した後、30℃まで冷却して三層構
造のフィルムを得た。
On the other hand, a polypropylene random copolymer having an MFR of 4 g/10 minutes, ethylene of 5% by weight, and propylene of 95% by weight and 96% by weight was extruded through the dies of two extruders set at 250°C, and the above! ) is laminated on both sides of the film, and then
Stretched 9 times in the transverse direction at a temperature of 155°C to 162°C.
After annealing at 30° C., the film was cooled to 30° C. to obtain a three-layer film.

3)印刷及び接着層(1d)の製造 上記三層構造の積層フィルムの両側にコロナ放電処理を
施した後、アクリル系帯電防止剤とポリエチレンイミン
が配合された水溶液を0.1g/ゴの塗工量となる様に
塗布した。この基材層(A)の片面に容器の内容物、商
品名、成分、製造元、販売元などをグラビアインキで印
刷した後、この印刷面に低密度のポリエチレン(三菱ポ
リエチLK−40)を230℃に設定された押出機のダ
イより20μtmの膜厚となるようにラミネートして接
着層を施したフィルムを得た。このフィルムの物性を第
1表に示す。
3) Printing and production of adhesive layer (1d) After corona discharge treatment was applied to both sides of the above three-layer laminated film, an aqueous solution containing an acrylic antistatic agent and polyethyleneimine was applied at a rate of 0.1 g/g. It was applied to achieve the required amount of work. After printing the contents of the container, product name, ingredients, manufacturer, distributor, etc. on one side of this base layer (A) with gravure ink, low density polyethylene (Mitsubishi Polyethylene LK-40) is applied to the printed side at 230 mm. A film with an adhesive layer was obtained by laminating the film to a thickness of 20 μtm through the die of an extruder set at .degree. The physical properties of this film are shown in Table 1.

【図面の簡単な説明】[Brief explanation of drawings]

第1図は本発明実施例のラベル付き中空成形容器の製造
方法において用いた成形機の断面図である。 1・・・ラベル、1a・・・基材層、1b・・・表面層
、1C・・裏面層、1d・・・接着層、2・・・中空成
形容器製造用成形機、3・・・金型、3a・・・金型内
壁、4・・・ダイ、5・・・パリソン、5a・・・パリ
ソンの外面、6・・・ノズル。
FIG. 1 is a sectional view of a molding machine used in the method for manufacturing a labeled blow-molded container according to an embodiment of the present invention. DESCRIPTION OF SYMBOLS 1... Label, 1a... Base material layer, 1b... Surface layer, 1C... Back layer, 1d... Adhesive layer, 2... Molding machine for blow molded container manufacturing, 3... Mold, 3a...Mold inner wall, 4...Die, 5...Parison, 5a...Outer surface of parison, 6...Nozzle.

Claims (1)

【特許請求の範囲】 1、厚さが50〜250μtmで、不透明度が10%以
下、縦方向及び横方向のクラーク剛度が2〜15の樹脂
フィルムより形成されていることを特徴とする、透明な
インモールド用ラベル。 2、樹脂フィルムが、ラベル全体の肉厚の 15%〜50%未満を占め、引張弾性率 8,000〜40,000kg/cm^2の基材層と、
該基材層の少なくとも片面に積層したラベル全体の肉厚
の50〜85%を占め、引張弾性率 2,000〜6,000kg/cm^2の弾性樹脂層と
からなる請求項1に記載の透明なインモールド用ラベル
。 3、樹脂フィルムが、ラベル全体の肉厚の 15%〜50%未満を占め、引張弾性率 8,000〜40,000kg/cm^2の基材層と、
該基材層の少なくとも片面に積層したラベル全体の肉厚
の50〜85%を占め、引張弾性率 2,000〜6,000kg/cm^2の弾性樹脂層と
、該弾性樹脂層の前記基材層と反対の側の面に積層した
ラベル全体の肉厚の0.1〜5%を占め、該基材層を形
成する樹脂の融点よりも10℃以上低い融点を有する樹
脂より形成された接着層とから構成されたものである請
求項1に記載の透明なインモールド用ラベル。
[Claims] 1. A transparent resin film having a thickness of 50 to 250 μtm, an opacity of 10% or less, and a Clark stiffness of 2 to 15 in the longitudinal and lateral directions. In-mold label. 2. A base material layer in which the resin film occupies 15% to less than 50% of the wall thickness of the entire label and has a tensile modulus of 8,000 to 40,000 kg/cm^2;
2. An elastic resin layer according to claim 1, comprising an elastic resin layer laminated on at least one side of the base material layer and accounting for 50 to 85% of the thickness of the entire label and having a tensile modulus of elasticity of 2,000 to 6,000 kg/cm^2. Transparent in-mold label. 3. A base material layer in which the resin film occupies 15% to less than 50% of the wall thickness of the entire label and has a tensile modulus of 8,000 to 40,000 kg/cm^2;
an elastic resin layer laminated on at least one side of the base material layer, which occupies 50 to 85% of the total wall thickness of the label and has a tensile modulus of elasticity of 2,000 to 6,000 kg/cm^2; and the base layer of the elastic resin layer. It is made of a resin that accounts for 0.1 to 5% of the total thickness of the label laminated on the side opposite to the material layer and has a melting point that is 10°C or more lower than the melting point of the resin that forms the base material layer. The transparent in-mold label according to claim 1, comprising an adhesive layer.
JP2104107A 1990-04-19 1990-04-19 Transparent in-mold label Expired - Lifetime JP2848916B2 (en)