JPH0446987B2 - - Google Patents

Info

Publication number
JPH0446987B2
JPH0446987B2 JP23510685A JP23510685A JPH0446987B2 JP H0446987 B2 JPH0446987 B2 JP H0446987B2 JP 23510685 A JP23510685 A JP 23510685A JP 23510685 A JP23510685 A JP 23510685A JP H0446987 B2 JPH0446987 B2 JP H0446987B2
Authority
JP
Japan
Prior art keywords
acid
weight
polyether ester
carbon atoms
polyamide
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
JP23510685A
Other languages
Japanese (ja)
Other versions
JPS6295340A (en
Inventor
Keiji Kayaba
Satoru Mori
Yoshuki Yamamoto
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toray Industries Inc
Original Assignee
Toray Industries Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toray Industries Inc filed Critical Toray Industries Inc
Priority to JP23510685A priority Critical patent/JPS6295340A/en
Publication of JPS6295340A publication Critical patent/JPS6295340A/en
Publication of JPH0446987B2 publication Critical patent/JPH0446987B2/ja
Granted legal-status Critical Current

Description

【発明の詳細な説明】[Detailed description of the invention]

<産業上の利用分野> 本発明は、成形性とゴム特性のすぐれたポリエ
ーテルエステルアミド成形用樹脂組成物に関する
ものである。 <従来の技術> ポリマー主鎖中にポリアミド繰返し単位、ポリ
エーテル繰返し単位およびエステル結合を有する
ポリエーテルエステルアミドは公知である。(米
国特許第3044987号明細書) <発明が解決しようとする問題点> ポリエーテルエステルアミドは柔軟性、軽量
性、透明性、低温耐衝撃性にすぐれるため各種成
形用等に有用されているが、時計の消音ギヤ、パ
ツキンなど小型成形品、薄葉成形品を射出成形し
た場合には、ポリアミドハード成分の結晶化のた
め流動性を低下し、シヨートシヨツトや未充填の
成形品が得られる問題が指摘されている。この問
題を解決する方法として低い重合度のポリエーテ
ルエステルアミドを使用する方法、成形温度を高
くしてポリエーテルエステルアミドの溶融粘度を
下げる方法が考えられる。低重合度のポリエーテ
ルエステルアミドを用いる場合には、得られた成
形品の屈曲疲労に代表されるゴム特性が悪く、又
高温の成形温度でポリエーテルエステルアミドを
成形する場合には、ポリ(アルキレンオキシド)
グリコールのソフト成分の耐熱性が劣るため熱分
解して重合度が低下し、同様にゴム特性が悪くな
る。又低重合度のポリエーテルエステルアミドを
用いる方法、成形温度を高くする方法は、本質的
に成形品にバリが発生しやすい問題がある。 本発明は、上述の問題点を解決し、短い成形サ
イクルで優れた成形品を得るために成形加工性が
改善され、又得られた成形品が優れたゴム特性を
有する成形用組成物の提供を目的とする。 <問題点を解決するための手段> 本発明の上記の目的は、炭素原子数6以上のア
ミノカルボン酸またはラクタム、もしくは炭素数
6以上のジアミンとジカルボン酸の塩から誘導さ
れるポリアミドをハード成分としてX重量%含有
し、数平均分子量300〜6000のポリ(アルキレン
オキシド)グリコールおよび炭素原子数4〜20の
ジカルボン酸から誘導されるポリエーテルエステ
ルをソフト成分として100−X重量%含有するポ
リエーテルエステルアミド(A)1〜99重量%と、炭
素原子数6以上のアミノカルボン酸またはラクタ
ム、もしくは炭素数6以上のジアミンとジカルボ
ン酸の塩から誘導されるポリアミドをハード成分
としてY重量%含有し、数平均分子量300〜6000
のポリ(アルキレンオキシド)グリコールおよび
炭素原子数4〜20のジカルボン酸から誘導される
ポリエーテルエステルをソフト成分として100−
Y重量%含有するポリエーテルエステルアミド(B)
99〜1重量%とからなり、XとYが 2≦|X−Y|≦60 の範囲にあることを特徴とするポリエーテルエス
テルアミド成形用樹脂組成物とすることによつて
達成されることがわかつた。 以下本発明の構成を述べる。 本発明のポリエーテルエステルアミド(A)及び(B)
における炭素数が6以上のアミノカルボン酸また
はラクタムもしくは炭素数6以上のジアミンとジ
カルボン酸の塩としては、ω−アミノカルボン
酸、ω−アミノエナント酸、ω−アミノカプリル
酸、ω−アミノペラルゴン酸、ω−アミノカプリ
ン酸、11−アミノウンデカン酸、12−アミノドデ
カン酸等のアミノカルボン酸あるいはカプロラク
タム、エナントラクタム、カプリルラクタム、ラ
ウロラクタム等のラクタムおよびヘキサメチレン
ジアミン−アジピン酸塩、ヘキサメチレンジアミ
ン−セバシン酸塩、ヘキサメチレンジアミン−イ
ソフタル酸塩、ウンデカメチレンジアミン−アジ
ピン酸塩、4,4′−ジアミノジシクロヘキシルメ
タン−ドデカンジ酸塩などのジアミン−ジカルボ
ン酸の塩があるが、特に11−アミノウンデカン
酸、12−アミノドデカン酸が好ましく、目的と用
途に応じてはこれらを併用することもできる。 またポリエーテルエステルアミドの融点を下げ
たり、接着性を高めるなどの目的でその他のアミ
ド形成性成分を共重合成分として用いることも少
量範囲なら許容される。 本発明のポリエーテルエステルアミド(A)及び(B)
における数平均分子量が300〜6000のポリ(アル
キレンオキシド)グリコールとしては、ポリエチ
レングリコール、ポリ(1,2−および1,3−
プロピレンオキシド)グリコール、ポリ(テトラ
メチレンオキシド)グリコール、ポリ(ヘキサメ
チレンオキシド)グリコール、エチレンオキシド
とプロピレンオキシドのブロツク又はランダム共
重合体、エチレンオキシドとテトラヒドロフラン
のブロツク又はランダム共重合体などが挙げら
れ、就中耐熱性、耐水性、機械的強度、弾性回復
性など、すぐれたポリエーテルエステルアミドの
物理的性質からポリ(テトラメチレンオキシド)
グリコールが好ましく用いられる。ポリ(アルキ
レンオキシド)グリコールの数平均分子量は300
〜600の範囲で用いうるが、重合時に粗大な相分
離を起こさず、低温特性や機械的性質がすぐれる
分子量領域が選択され、この最適分子量領域はポ
リ(アルキレンオキシド)グリコールの種類によ
つて異なる。例えばポリエチレングリコールの場
合300〜6000、特に好ましくは1000〜4000が、ポ
リ(プロピレンオキシド)グリコールの場合300
〜5000、特に好ましくは500〜3000が、またポリ
(テトラメチレンオキシド)グリコールの場合500
〜3000、特に好ましくは500〜2500の分子量領域
のものが好ましく用いられる。 本発明のポリエーテルエステルアミド(A)及び(B)
における炭素数4〜20のジカルボン酸としてはテ
レフタル酸、イソフタル酸、ナフタレン−2,6
−ジカルボン酸、ナフタレン−2,7−ジカルボ
ン酸、ジフエニル−4,4′−ジカルボン酸、ジフ
エノキシエタンジカルボン酸、3−スルホイソフ
タル酸ナトリウムのごとき芳香族ジカルボン酸、
1,4−シクロヘキサンジカルボン酸、1,2−
シクロヘキサンジカルボン酸、ジシクロヘキシル
−4,4′−ジカルボン酸のごとき脂環族ジカルボ
ン酸、およびコハク酸、シユウ酸、アジピン酸、
セバシン酸、ドデカンジ酸(デカンジカルボン
酸)のごとき脂肪族ジカルボン酸を挙げることが
できる。特にテレフタル酸、イソフタル酸、1,
4−シクロヘキサンジカルボン酸、アジピン酸、
セバシン酸、ドデカンジ酸のようなジカルボン酸
が重合性、色調およびポリマの物理的性質の点点
から好ましく用いられる。 本発明においては、ポリエーテルエステルアミ
ド(A)及び(B)におけるハード成分のポリアミドの含
有量およびYは 2≦|X−Y|≦60 であることが必要であり、 好ましくは 4≦|X−Y|≦30 である。 |X−Y|が2未満では成形用組成物とした場
合の成形性向上効果が小さく、又60を越えると(A)
ポリマーと(B)ポリマーの相溶性が低下して粗大相
分離構造を形成し、ゴム特性が低下し、又成形品
が真珠光沢を呈するため使用できない。 また、本発明ではポリエーテルエステルアミド
(A)及び(B)の配合比は(A)1〜99重量%に対し(B)99〜
1重量%にする必要があり、好ましくは(A)5〜95
重量%に対し(B)95〜5重量%である。少量成分が
1重量%未満では成形性、ゴム特性の改良効果が
小さすぎるからである。 更に、本発明の効果が就中最も顕著に示される
ためには、ポリエーテルエステルアミド(A)及び(B)
におけるハード成分のポリアミドの含有量X及び
Yは 10≦X≦95 10≦Y≦95 (X,Y:重量%) の範囲にあることが好ましい。X及びYの値が10
未満の場合には得られたポリエーテルエステルア
ミドの高温特性、機械的性質、成形性が十分でな
くなり、逆に95を越えるとゴム特性が低下する傾
向がある。 ここで、ポリエーテルエステルアミド中のポリ
アミド成分の含有量XおよびYは、アミド基(−
CONH−)の固有振動数(1640-1cm)を利用し
て、赤外吸収スペクトル(IR)から以下のよう
にして求めることができる。 すなわち、予めポリアミド/ポリエーテルエス
テル組成比が既知のポリマ3〜5水準(異種の組
成比からなるフイルム状試料)を用いて、各組成
比におけるポリアミド成分含有量と吸光度との関
係から検量線を作成しておく。 そして、測定すべき試料フイルムについて、固
有振動数(1640-1cm)の吸収スペクトルから吸光
度を求め、この結果を上記の検量線に外挿するこ
とによつて、ポリアミド成分の含有量XおよびY
を容易に求めることができ、さらにはこのポリア
ミド成分の含有量XおよびYを、それぞれ100重
量%から減ずることによつて、ポリエーテルエス
テル成分の含有量とすることができる。 なお、ポリエーテルエステルアミドの縮重合を
十分行えば、得られるポリマー中のポリアミド成
分とポリエーテルエステル成分の比は、仕込み原
料におけるポリアミド成分とポリエーテルエステ
ル成分の割合とほぼ一致することが確認されてい
る。 また、ポリエーテルエステルアミド(A)及び(B)の
重合方法は特に限定されず公知の方法を利用する
ことができる。たとえば、アミノカルボン酸また
はラクタム、もしくはジアミンとジカルボン酸の
塩(a)とジカルボン酸(c)を反応させて両末端がカル
ボン酸基のポリアミドプレポリマをつくりこれに
ポリ(アルキレンオキシド)グリコール(b)を真空
下に反応させる方法、あるいは上記(a)、(b)、(c)の
化合物を反応槽に仕込み、水の存在下または不存
在下に高温で加熱反応させることによりカルボン
酸末端のポリアミドプレポリマを生成させ、その
後、常圧または減圧下で重合を進める方法が知ら
れている。また、上記(a)、(b)、(c)の化合物を同時
に反応槽に仕込み、溶融重合したのち、高真空下
で一挙に重合をすすめる方法もあり、むしろこの
方法がポリマの着色も少なく好ましい。 本発明の組成物は、通常2種類のポリエーテル
エステルアミドを溶融混合するものであるが、溶
融混合の方法は特に限定されない。たとえば押出
機を使用して混合してもよいし、二種のペレツト
をドライブレンドし、射出、押出成形することも
可能である。また本発明の成形用組成物には、本
発明の目的を損なわない限りにおいて他の成分、
たとえば顔料、染料、難燃剤、耐熱剤、酸化防止
剤、耐候剤、滑剤、離型剤、帯電防止剤、可塑
剤、結晶核剤、発泡剤、強化剤、充填剤および他
の重合体など添加することが可能である。 <実施例> 実施例中特にことわらない限り、部数は重量部
を意味する。 参考例 ポリエーテルエステルアミドの重合 表1に示した割合のω−アミノドデカン酸
(ADA)、テレフタル酸(TPA)、及びポリ(テ
トラメチレンオキシド)グリコール(PTMG)
を“イルガノツクス”1098 0.5部(酸化防止剤)
と共にヘリカルリボン撹拌翼を備えた反応容器に
仕込み、窒素パージして260℃で1時間加熱撹拌
して均質透明溶液とした後、三酸化アンチモン触
媒0.015部、モノブチルモノヒドロキシ錫オキシ
ド触媒0.015部、りん酸0.005部(着色防止剤)を
添加し、減圧プログラムに従つて1時間で1mm
Hg以下の重合条件にもたらした。この条件にて
所定の重合度まで反応させると粘ちような無色透
明の溶融ポリマーが得られ、このポリマーをガツ
トとして水中に吐出すると結晶化して白化した。
得られたポリエーテルエステルアミドについて、
IR分析によるポリアミド成分の含有量、および
相対粘度、融点、結晶化温度の各測定結果を表1
に示す。 実施例1〜6、比較例1〜10 表2に示した配合組成になるように、参考例で
得たポリエーテルエステルアミド2種をドライブ
レンドし、(比較例1〜8についてはドライブレ
ンドせずに)5−オンスの射出能力を有する射出
成形機を使用して、射出温度220℃、金型温度40
℃で100×100×1mm大の角板を成形した。この
時、ポリマの流動性の尺度として成形下限圧を、
固化速度の尺度として成形サイクルを観察した。 この角板から25×100×1mm大の試験片を切り
出し、JIS K6301に記載された方法で、屈曲疲労
性を測定した。 結果をまとめて表2に示す。
<Industrial Application Field> The present invention relates to a polyether ester amide molding resin composition with excellent moldability and rubber properties. <Prior Art> Polyetheresteramides having polyamide repeating units, polyether repeating units and ester bonds in the polymer main chain are known. (U.S. Patent No. 3,044,987) <Problems to be solved by the invention> Polyetheresteramide is useful for various molding applications because it has excellent flexibility, lightness, transparency, and low-temperature impact resistance. However, when injection molding small molded products such as silencer gears and gaskets for watches, or thin-film molded products, the fluidity decreases due to crystallization of the polyamide hard component, resulting in short shots or unfilled molded products. It has been pointed out. Possible ways to solve this problem include using polyether ester amide with a low degree of polymerization and increasing the molding temperature to lower the melt viscosity of the polyether ester amide. When polyether ester amide with a low degree of polymerization is used, the rubber properties of the resulting molded product, typified by bending fatigue, are poor, and when polyether ester amide is molded at a high molding temperature, poly( alkylene oxide)
Since the soft component of glycol has poor heat resistance, it decomposes thermally and the degree of polymerization decreases, which also deteriorates the rubber properties. Furthermore, methods using polyether ester amide with a low degree of polymerization and methods in which the molding temperature is increased inherently have the problem that burrs are likely to occur in the molded product. The present invention solves the above-mentioned problems and provides a molding composition with improved molding processability in order to obtain an excellent molded product in a short molding cycle, and in which the obtained molded product has excellent rubber properties. With the goal. <Means for Solving the Problems> The above-mentioned object of the present invention is to use a polyamide derived from an aminocarboxylic acid or lactam having 6 or more carbon atoms, or a salt of a diamine and dicarboxylic acid having 6 or more carbon atoms as a hard component. A polyether containing 100-X weight% of a polyether ester derived from a poly(alkylene oxide) glycol having a number average molecular weight of 300 to 6000 and a dicarboxylic acid having 4 to 20 carbon atoms as a soft component. Contains 1 to 99% by weight of ester amide (A) and Y% by weight of polyamide derived from an aminocarboxylic acid or lactam having 6 or more carbon atoms, or a salt of diamine and dicarboxylic acid having 6 or more carbon atoms as hard components. , number average molecular weight 300-6000
100-
Polyether ester amide (B) containing Y% by weight
99 to 1% by weight, and wherein X and Y are in the range of 2≦|X−Y|≦60. I understood. The configuration of the present invention will be described below. Polyetheresteramides (A) and (B) of the present invention
The salts of aminocarboxylic acids or lactams having 6 or more carbon atoms or diamines and dicarboxylic acids having 6 or more carbon atoms include ω-aminocarboxylic acid, ω-aminoenanthic acid, ω-aminocaprylic acid, ω-aminopelargonic acid. , aminocarboxylic acids such as ω-aminocapric acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid, or lactams such as caprolactam, enantholactam, capryllactam, laurolactam, and hexamethylenediamine adipate, hexamethylenediamine- Salts of diamine-dicarboxylic acids such as sebacate, hexamethylenediamine-isophthalate, undecamethylenediamine-adipate, 4,4'-diaminodicyclohexylmethane-dodecanedioate, but especially 11-aminoundecane Acid, 12-aminododecanoic acid is preferred, and these may be used in combination depending on the purpose and use. It is also permissible to use other amide-forming components as copolymerization components in small amounts for the purpose of lowering the melting point of polyether ester amide or increasing adhesiveness. Polyetheresteramides (A) and (B) of the present invention
Examples of poly(alkylene oxide) glycols having a number average molecular weight of 300 to 6,000 include polyethylene glycol, poly(1,2- and 1,3-
Propylene oxide) glycol, poly(tetramethylene oxide) glycol, poly(hexamethylene oxide) glycol, block or random copolymers of ethylene oxide and propylene oxide, block or random copolymers of ethylene oxide and tetrahydrofuran, etc., among others. Poly(tetramethylene oxide) due to the excellent physical properties of polyether esteramide, such as heat resistance, water resistance, mechanical strength, and elastic recovery.
Glycols are preferably used. The number average molecular weight of poly(alkylene oxide) glycol is 300
~600, but a molecular weight range that does not cause coarse phase separation during polymerization and has excellent low temperature properties and mechanical properties is selected, and this optimum molecular weight range depends on the type of poly(alkylene oxide) glycol. different. For example, 300-6000 for polyethylene glycol, particularly preferably 1000-4000, and 300 for poly(propylene oxide) glycol.
~5000, particularly preferably 500-3000, but also 500 in the case of poly(tetramethylene oxide) glycol
Those having a molecular weight in the range of 3,000 to 3,000, particularly preferably 500 to 2,500 are preferably used. Polyetheresteramides (A) and (B) of the present invention
Examples of dicarboxylic acids having 4 to 20 carbon atoms include terephthalic acid, isophthalic acid, and naphthalene-2,6
- aromatic dicarboxylic acids such as dicarboxylic acid, naphthalene-2,7-dicarboxylic acid, diphenyl-4,4'-dicarboxylic acid, diphenoxyethane dicarboxylic acid, sodium 3-sulfoisophthalate,
1,4-cyclohexanedicarboxylic acid, 1,2-
Alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid, dicyclohexyl-4,4'-dicarboxylic acid, and succinic acid, oxalic acid, adipic acid,
Mention may be made of aliphatic dicarboxylic acids such as sebacic acid and dodecanedioic acid (decanedicarboxylic acid). Especially terephthalic acid, isophthalic acid, 1,
4-cyclohexanedicarboxylic acid, adipic acid,
Dicarboxylic acids such as sebacic acid and dodecanedioic acid are preferably used from the viewpoint of polymerizability, color tone, and physical properties of the polymer. In the present invention, the content of the hard component polyamide and Y in the polyetheresteramides (A) and (B) must be 2≦|X−Y|≦60, preferably 4≦|X -Y|≦30. If |X-Y| is less than 2, the moldability improvement effect when used as a molding composition is small, and if it exceeds 60, (A)
The compatibility between the polymer and the (B) polymer decreases, forming a coarse phase-separated structure, resulting in decreased rubber properties and the molded product exhibiting pearlescent luster, making it unusable. In addition, in the present invention, polyether ester amide
The blending ratio of (A) and (B) is (A) 1 to 99% by weight and (B) 99 to 99% by weight.
It is necessary to make it 1% by weight, preferably (A) 5-95
(B) is 95 to 5% by weight. This is because if the minor component is less than 1% by weight, the effect of improving moldability and rubber properties is too small. Furthermore, in order for the effects of the present invention to be exhibited most notably, polyether ester amides (A) and (B)
It is preferable that the contents X and Y of the polyamide of the hard component in are in the following ranges: 10≦X≦95 10≦Y≦95 (X, Y: weight %). X and Y values are 10
If it is less than 95, the high-temperature properties, mechanical properties, and moldability of the resulting polyether ester amide will be insufficient, while if it exceeds 95, the rubber properties will tend to deteriorate. Here, the contents X and Y of the polyamide component in the polyetheresteramide are amide groups (-
It can be determined from the infrared absorption spectrum (IR) as follows using the natural frequency (1640 -1 cm) of CONH-). That is, using 3 to 5 levels of polymers (film samples with different composition ratios) whose polyamide/polyetherester composition ratios are known in advance, a calibration curve is drawn from the relationship between the polyamide component content and absorbance at each composition ratio. Create it. Then, for the sample film to be measured, the absorbance is determined from the absorption spectrum at the natural frequency (1640 -1 cm), and by extrapolating this result to the above calibration curve, the content of the polyamide component X and Y
can be easily determined, and by subtracting the contents X and Y of the polyamide component from 100% by weight, respectively, the content of the polyetherester component can be determined. It has been confirmed that if polycondensation of polyether ester amide is carried out sufficiently, the ratio of the polyamide component to the polyether ester component in the resulting polymer will almost match the ratio of the polyamide component to the polyether ester component in the raw materials. ing. Furthermore, the method for polymerizing the polyetheresteramides (A) and (B) is not particularly limited, and any known method can be used. For example, a polyamide prepolymer with carboxylic acid groups at both ends is produced by reacting an aminocarboxylic acid or a lactam, or a salt of a diamine and a dicarboxylic acid (a) with a dicarboxylic acid (c), which is then injected with poly(alkylene oxide) glycol (b). ) under vacuum, or by charging the compounds (a), (b), and (c) above into a reaction tank and heating them to react at high temperature in the presence or absence of water. A method is known in which a polyamide prepolymer is produced and then polymerization is proceeded under normal pressure or reduced pressure. There is also a method in which the compounds (a), (b), and (c) above are charged into a reaction tank at the same time, melt-polymerized, and then polymerized all at once under high vacuum; this method actually causes less coloring of the polymer. preferable. The composition of the present invention is usually prepared by melt-mixing two types of polyether ester amides, but the method of melt-mixing is not particularly limited. For example, mixing may be performed using an extruder, or two types of pellets may be dry blended and then injection molded or extruded. In addition, the molding composition of the present invention may contain other components as long as they do not impair the purpose of the present invention.
For example, additives such as pigments, dyes, flame retardants, heat resistant agents, antioxidants, weathering agents, lubricants, mold release agents, antistatic agents, plasticizers, nucleating agents, blowing agents, reinforcing agents, fillers and other polymers. It is possible to do so. <Examples> Unless otherwise specified in the examples, parts mean parts by weight. Reference example Polymerization of polyether ester amide ω-aminododecanoic acid (ADA), terephthalic acid (TPA), and poly(tetramethylene oxide) glycol (PTMG) in the proportions shown in Table 1
“Irganox” 1098 0.5 part (antioxidant)
The mixture was charged into a reaction vessel equipped with a helical ribbon stirring blade, purged with nitrogen, heated and stirred at 260°C for 1 hour to obtain a homogeneous transparent solution, and then mixed with 0.015 parts of antimony trioxide catalyst, 0.015 parts of monobutyl monohydroxytin oxide catalyst, Add 0.005 parts of phosphoric acid (anti-coloring agent) and follow the vacuum program to 1 mm in 1 hour.
The polymerization conditions were brought to below Hg. When the reaction was carried out under these conditions to a predetermined degree of polymerization, a viscous colorless and transparent molten polymer was obtained, and when this polymer was discharged into water as a gut, it crystallized and turned white.
Regarding the obtained polyether ester amide,
Table 1 shows the measurement results of polyamide component content, relative viscosity, melting point, and crystallization temperature by IR analysis.
Shown below. Examples 1 to 6, Comparative Examples 1 to 10 Two types of polyether ester amides obtained in Reference Examples were dry blended to have the composition shown in Table 2 (for Comparative Examples 1 to 8, dry blending was performed). ) Using an injection molding machine with a 5-ounce injection capacity, the injection temperature was 220℃ and the mold temperature was 40℃.
A square plate measuring 100 x 100 x 1 mm was formed at ℃. At this time, the lower limit pressure for molding is used as a measure of the fluidity of the polymer.
Molding cycles were observed as a measure of solidification rate. A test piece measuring 25 x 100 x 1 mm was cut out from this square plate, and its bending fatigue strength was measured by the method described in JIS K6301. The results are summarized in Table 2.

【表】【table】

【表】 表1、2から次のことがわかる。 たとえば実施例3(ポリアミド含有量35%、|X
−Y|=20)と比較例4、5(ポリアミド含有量
30、45%)において、 成形下限圧:実施例3<比較例4、5 成形サイクル:実施例3<比較例4、5 亀裂成長長さ:実施例3<比較例4、5 でありいずれも実施例3が優れている。 また、比較例9(ポリアミド含有量25.5%|X
−Y|=1)は比較例2、3(ポリアミド含有量
25、26%)とほぼ同等の成形性、屈曲疲労性を示
し、改良効果がみられない。さらに比較例10(ポ
リアミド含有量57.5%、|X−Y|=65)は比較
例6(ポリアミド含有量55%)より成形性、屈曲
疲労性が劣る。 <発明の効果> 本発明の樹脂組成物は、組成の異なるポリエー
テルエステルアミドを混合するためポリエーテル
エステルアミド共重合体単独のものと比較し、成
形性、ゴム特性が極めて優れるものである。
[Table] The following can be seen from Tables 1 and 2. For example, Example 3 (polyamide content 35%, |
-Y|=20) and Comparative Examples 4 and 5 (polyamide content
30, 45%), lower limit molding pressure: Example 3 < Comparative Examples 4, 5 Molding cycle: Example 3 < Comparative Examples 4, 5 Crack growth length: Example 3 < Comparative Examples 4, 5 Example 3 is superior. In addition, Comparative Example 9 (polyamide content 25.5% |
-Y|=1) is Comparative Examples 2 and 3 (polyamide content
25, 26%), showing almost the same formability and bending fatigue resistance, and no improvement effect was observed. Furthermore, Comparative Example 10 (polyamide content 57.5%, |X-Y|=65) is inferior to Comparative Example 6 (polyamide content 55%) in moldability and bending fatigue resistance. <Effects of the Invention> Since the resin composition of the present invention is a mixture of polyetheresteramides having different compositions, it has extremely superior moldability and rubber properties compared to a single polyetheresteramide copolymer.

Claims (1)

【特許請求の範囲】 1 炭素原子数6以上のアミノカルボン酸または
ラクタム、もしくは炭素数6以上のジアミンとジ
カルボン酸の塩から誘導されるポリアミドをハー
ド成分としてX重量%含有し、数平均分子量300
〜6000のポリ(アルキレンオキシド)グリコール
および炭素原子数4〜20のジカルボン酸から誘導
されるポリエーテルエステルをソフト成分として
100−X重量%含有するポリエーテルエステルア
ミド(A)1〜99重量%と、炭素原子数6以上のアミ
ノカルボン酸またはラクタム、もしくは炭素数6
以上のジアミンとジカルボン酸の塩から誘導され
るポリアミドをハード成分としてY重量%含有
し、数平均分子量300〜6000のポリ(アルキレン
オキシド)グリコールおよび炭素原子数4〜20の
ジカルボン酸から誘導されるポリエーテルエステ
ルをソフト成分として100−Y重量%含有するポ
リエーテルエステルアミド(B)99〜1重量%とから
なり、XとYが 2≦|X−Y|≦60 の範囲にあることを特徴とするポリエーテルエス
テルアミド成形用樹脂組成物。
[Scope of Claims] 1. A polyamide derived from an aminocarboxylic acid or lactam having 6 or more carbon atoms, or a salt of diamine and dicarboxylic acid having 6 or more carbon atoms as a hard component, containing X weight %, and having a number average molecular weight of 300.
~6000 poly(alkylene oxide) glycol and polyether ester derived from C4-20 dicarboxylic acid as soft component
1 to 99% by weight of polyether ester amide (A) containing 100-X% by weight, and an aminocarboxylic acid or lactam having 6 or more carbon atoms, or 6 carbon atoms
Contains Y% by weight of polyamide derived from the above diamine and dicarboxylic acid salt as a hard component, and is derived from poly(alkylene oxide) glycol having a number average molecular weight of 300 to 6000 and a dicarboxylic acid having 4 to 20 carbon atoms. It consists of 99 to 1% by weight of polyetherester amide (B) containing 100-Y% by weight of polyetherester as a soft component, and is characterized in that X and Y are in the range of 2≦|X-Y|≦60. A polyether ester amide molding resin composition.
JP23510685A 1985-10-23 1985-10-23 Polyether ester amide molding resin composition Granted JPS6295340A (en)