JPH0448083A - Corrosion and wear resistant material having high strength and its production - Google Patents

Corrosion and wear resistant material having high strength and its production

Info

Publication number
JPH0448083A
JPH0448083A JP15532190A JP15532190A JPH0448083A JP H0448083 A JPH0448083 A JP H0448083A JP 15532190 A JP15532190 A JP 15532190A JP 15532190 A JP15532190 A JP 15532190A JP H0448083 A JPH0448083 A JP H0448083A
Authority
JP
Japan
Prior art keywords
particles
composite layer
based alloy
alloy
resistant
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP15532190A
Other languages
Japanese (ja)
Inventor
Kimitaka Maruyama
公孝 丸山
Naotaka Kawaguchi
川口 直孝
Mikiyoshi Miyauchi
宮内 幹由
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shibaura Machine Co Ltd
Original Assignee
Toshiba Machine Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toshiba Machine Co Ltd filed Critical Toshiba Machine Co Ltd
Priority to JP15532190A priority Critical patent/JPH0448083A/en
Publication of JPH0448083A publication Critical patent/JPH0448083A/en
Pending legal-status Critical Current

Abstract

PURPOSE:To produce a corrosion and wear resistant material having high strength by joining a composite layer contg. hard particles of carbide, metal particles for regulating physical properties and an Fe-based alloy as a matrix metal to the surface of a base material. CONSTITUTION:Hard particles of one or more among carbide, boride and nitride are mixed with metal particles as particles for regulating physical properties and the mixed particles are fixed on the surface of a base material. One or more among Fe-, Ni- and Co-based alloys as a matrix metal are set in contact with the mixed particles and heated with a heating source. The matrix metal is melted and allowed to penetrate into the gaps among the mixed particles to form a composite layer and this layer is diffused and joined to the surface of the base material. Particles of one or more among Fe-, Ni-, Co- and Cu-based alloys are suitable for use as the particles for regulating physical properties.

Description

【発明の詳細な説明】 [産業上の利用分野コ 本発明は、機械部材に耐蝕耐摩耗性材料を被覆する技術
に関し、更に詳しくは、特にプラスチック成形機のバレ
ル、スクリュー等に用いられる耐蝕耐摩耗性材料の強度
・靭性の向上を図る高強度耐14!ift摩耗性材料お
よびその製造方法に関する。
DETAILED DESCRIPTION OF THE INVENTION [Field of Industrial Application] The present invention relates to a technique for coating mechanical parts with a corrosion-resistant and wear-resistant material. High strength resistance 14 to improve the strength and toughness of abrasive materials! Ift abrasive material and method for manufacturing the same.

[従来の技術] 機械部材に耐蝕耐摩耗性材料を被覆する技術として、従
来より、硬質粒子を基材表面形状に有機バインダ等を用
いて固定し、複合層のマトリックス金属を硬質粒子に接
触するように配置し、加熱してマトリックス金属を溶融
させるものが用いられていた。この種の技術の1つとし
て、例えば本出願人か特願昭61−196362号とし
て出願した炭化物または硼化物の粉末と有機バインダを
混練して母材に被覆し、同被覆層を機械加工した後、焼
結炉内で前記被覆層の前記有機バインダを加熱して除去
すると共に溶融した金属バインダを前記被覆層に浸透さ
せかつ母材と接合せしめる耐摩耗性材料の被覆方法を例
示す・ることかできる。この場合、溶融マトリックス金
属は、硬質粒子中に浸透し、複合層を形成すると共に基
材材料に接合する。
[Prior art] Conventionally, as a technique for coating mechanical parts with corrosion-resistant and wear-resistant materials, hard particles are fixed to the surface shape of the base material using an organic binder, etc., and the matrix metal of the composite layer is brought into contact with the hard particles. The matrix metal was placed in a similar manner and heated to melt the matrix metal. One technique of this kind is, for example, as disclosed by the present applicant in Japanese Patent Application No. 196362/1982, in which carbide or boride powder and an organic binder are kneaded and coated on a base material, and the coating layer is machined. Afterwards, the organic binder of the coating layer is heated and removed in a sintering furnace, and the molten metal binder is infiltrated into the coating layer and bonded to the base material. I can do it. In this case, the molten matrix metal penetrates into the hard particles, forming a composite layer and bonding to the substrate material.

しかしながら、この種の方法の問題点として、複合層の
物性は硬質粒子の量に大きく左右されるという問題があ
る0例えば、硬質粒子としてタングステンカーバイド粒
子(以下託と指称する)を用い、マトリックス金属とし
て1基合金の複合層を用いた場合である。
However, a problem with this type of method is that the physical properties of the composite layer are largely influenced by the amount of hard particles. This is a case where a composite layer of a single alloy is used.

有機バインダにより甑を基材表面に固定させる方法とし
て、静水圧あるいはスプレ一方式等かあるか、この場合
、讐Ciはその固定方法により決定され、これらの方法
では−C量は50〜60重量%程度である。更に、 ■この複合層の線膨張率は7〜8x10−’/”C程度
であり、基材の材料か制限され、また■複合層の機械的
性質も固定されるなめ、機械的性質の向上は非常に困難
になる 等の問題点があった。
Is there a method of fixing the moss to the surface of the substrate using an organic binder, such as hydrostatic pressure or spraying? In this case, the amount of -C is determined by the fixing method, and in these methods, the amount of -C is 50 to 60% by weight. It is about %. Furthermore, ■The coefficient of linear expansion of this composite layer is about 7 to 8 x 10-'/''C, which limits the base material, and ■The mechanical properties of the composite layer are also fixed, improving mechanical properties. There were problems such as making it extremely difficult.

このような方法に対し、複合層中に第3の物質として物
性調整粒子を添加すれば、線膨張率を調整することかで
き、また物性調整粒子を添加することにより、lAC量
を少なくすることができ、かつマトリックス金属を強く
することかできる結果、複合層の機械的性質を向上させ
ることかて゛きる可能性が考えられる。
In contrast to this method, if physical property adjusting particles are added as a third substance in the composite layer, the coefficient of linear expansion can be adjusted, and by adding physical property adjusting particles, the amount of lAC can be reduced. As a result of being able to strengthen the matrix metal, it is possible to improve the mechanical properties of the composite layer.

[発明が解決しようとする課題] 従来の技術においては、複合層の物性は硬質粒子とマト
リックス金属の種類とにより決定されていた。これに対
して本発明は、第3の物質として物性調整粒子を添加す
ることにより、複合層の物性を自由に調整することがで
き、硬質粒子の量を少くすると共にマトリックス金属の
強度の向上を図り、複合層の機械的性質の向上を実現す
ることのできる高強度耐蝕耐摩耗性材料およびその製造
方法を提供することを目的とする。
[Problems to be Solved by the Invention] In the prior art, the physical properties of the composite layer were determined by the hard particles and the type of matrix metal. In contrast, the present invention allows the physical properties of the composite layer to be adjusted freely by adding physical property adjusting particles as the third substance, thereby reducing the amount of hard particles and improving the strength of the matrix metal. The present invention aims to provide a high-strength corrosion-resistant and wear-resistant material that can improve the mechanical properties of a composite layer, and a method for manufacturing the same.

[課題を解決するための手段] 本発明によれは、複合層の硬質粒子として炭化物、硼化
物、窒化物の内少くとも1種以上と、複合層の物性調整
粒子として金属粒子と、複合層のマトリックス金属とし
てFe基合金、Ni基合金、Co基合金の内少くとも1
種以上とを含有する複合層を基材表面に接合させたこと
を特徴とする高強度耐蝕耐摩耗性材料が提供される。
[Means for Solving the Problems] According to the present invention, at least one of carbides, borides, and nitrides are used as hard particles of the composite layer, metal particles are used as the physical property adjusting particles of the composite layer, and metal particles are used as the physical property adjusting particles of the composite layer. As the matrix metal, at least one of Fe-based alloy, Ni-based alloy, and Co-based alloy is used.
Provided is a high-strength, corrosion-resistant and wear-resistant material characterized by having a composite layer containing at least one species bonded to the surface of a base material.

更に本発明によれは、複合層の硬質粒子として炭化物、
硼化物、窒化物の内少くとも1種以上と、複合層の物性
調整粒子として金属粒子とからなる混合粒子を基材表面
形状に固定し、更に前記混合粒子に接触するよう複合層
のマトリックス金属を配置しく複合層のマトリックス金
属としてFe基合金、Ni基合金、Co基合金の内少く
とも1種以上を含有する)、加熱源で加熱し、マトリッ
クス金属を溶融させ、混合粒子の間隙に浸透させて複合
層を形成すると共に基材表面に拡散接合させることを特
徴とする高強度耐蝕耐摩耗性材料の製造方法か提供され
る。
Furthermore, according to the present invention, carbide,
Mixed particles consisting of at least one of borides and nitrides and metal particles as physical property adjusting particles of the composite layer are fixed to the surface shape of the base material, and the matrix metal of the composite layer is further fixed to the surface shape of the base material so as to be in contact with the mixed particles. (containing at least one of Fe-based alloy, Ni-based alloy, and Co-based alloy as the matrix metal of the composite layer) is heated with a heat source to melt the matrix metal and penetrate into the gaps between the mixed particles. A method for producing a high-strength, corrosion-resistant and wear-resistant material is provided, which is characterized by forming a composite layer and diffusion bonding to the surface of a base material.

物性調整粒子が、Fe基合金、Ni基合金、Co基合金
、Cu合金の内少くとも1種以上からなるものであれば
好適である。
It is preferable that the physical property adjusting particles are made of at least one of Fe-based alloys, Ni-based alloys, Co-based alloys, and Cu alloys.

物性調整粒子か、複合層のマトリックス金属より融点の
高い合金粒子であれば好適である。
It is preferable to use physical property adjusting particles or alloy particles having a higher melting point than the matrix metal of the composite layer.

本発明の好適な態様として、複合層の硬質粒子としてW
Cを用い、物性調整粒子としてステンレス粒子の混合粉
を用い、これを有機バインダを用いて基材表面に固定し
、Ni基合金を混合粉層に接触するように配置し、真空
炉に挿入することにより、昇温過程で有機バインダが蒸
発分解し、更にNi基合金が溶融して混合粉層に浸透し
、複合層を形成すると共に基材に接合させる製造方法を
使用することができ、これにより優れた高強度耐蝕耐摩
耗性材料を得ることができる。
As a preferred embodiment of the present invention, W as the hard particles of the composite layer
Using C, a mixed powder of stainless steel particles is used as the physical property adjusting particles, this is fixed to the surface of the base material using an organic binder, the Ni-based alloy is placed in contact with the mixed powder layer, and the mixture is inserted into a vacuum furnace. This makes it possible to use a manufacturing method in which the organic binder evaporates and decomposes during the temperature raising process, and the Ni-based alloy melts and penetrates the mixed powder layer to form a composite layer and bond to the base material. As a result, a material with excellent high strength and corrosion resistance and wear resistance can be obtained.

[作用] 従来の技術においては、複合層の物性は硬質粒子の量に
大きく左右されるという問題があった。また、硬質粒子
の量はその固定方法により決定され、従来の方法では代
表的な硬質粒子である一C量は50〜60重量%程度で
あった。更に、従来の複合層のw&膨H率は7〜8X 
10−’/’C程度であり、基材の材料が制限され、ま
た複合層の機械的性質も固定されるため、機械的性質の
向上は非常に困離になる等の問題点があった。
[Function] In the conventional technology, there was a problem that the physical properties of the composite layer were largely influenced by the amount of hard particles. Further, the amount of hard particles is determined by the method of fixing them, and in the conventional method, the amount of 1C, which is a typical hard particle, was about 50 to 60% by weight. Furthermore, the W & expansion H ratio of the conventional composite layer is 7~8X
10-'/'C, the base material is limited, and the mechanical properties of the composite layer are also fixed, making it extremely difficult to improve the mechanical properties. .

すなわち、従来の技術においては、複合層の物性は硬質
粒子とマトリックス金属の種類とにより決定され、複合
層の物性を自由に調整することは極めて困難であった。
That is, in the conventional technology, the physical properties of the composite layer are determined by the hard particles and the type of matrix metal, and it is extremely difficult to freely adjust the physical properties of the composite layer.

本発明は、複合層中に第3の物質として物性調整粒子を
添加することにより、線膨脹率を調整し、さらに硬質粒
子の量を少なくすると共にマトリックス金属の強度向上
を実現するものである。これにより、複合層の機械的性
質を顕著に向上させることができる。
The present invention adjusts the linear expansion coefficient by adding physical property adjusting particles as a third substance to the composite layer, further reduces the amount of hard particles, and improves the strength of the matrix metal. This allows the mechanical properties of the composite layer to be significantly improved.

[発明の効果] 本発明によれば、複合層の硬質粒子および複合層のマト
リックス金属に加えて、第3の物質として物性調整粒子
を添加することにより、硬質粒子の量を少くすると共に
マトリックス金属の強度の向上を図り、複合層の8!械
的性質の向上を実現することのできる高強度耐蝕耐摩耗
性材料およびその製造方法が提供される。したがって本
発明によれば、物性調整粒子を添加することにより、耐
摩耗性を低下させることなく線膨脹率を大きくすること
かでき、かつ曲げ強度を大きくすることかできる。
[Effects of the Invention] According to the present invention, by adding physical property adjusting particles as a third substance in addition to the hard particles of the composite layer and the matrix metal of the composite layer, the amount of hard particles can be reduced and the matrix metal can be reduced. In order to improve the strength of the composite layer, 8! A high-strength corrosion-resistant and wear-resistant material capable of realizing improved mechanical properties and a method for producing the same are provided. Therefore, according to the present invention, by adding physical property adjusting particles, the coefficient of linear expansion can be increased without reducing the wear resistance, and the bending strength can also be increased.

[実施例] 以下に実施例により本発明を更に詳細に説明するが、本
発明は以下の実施例にのみ限定されるものではない。
[Examples] The present invention will be explained in more detail with reference to Examples below, but the present invention is not limited only to the following Examples.

裏1■ユ 複合層の硬質粒子として平均粒径10μmの甑を用い、
物性調整粒子として粒径30μmアンターの5US31
6および5US410粒子(後記するマトリックス金属
たる自溶性合金より融点が高い)を用い、これらを有機
バインダとするアクリル樹脂と有機溶剤とするメチル・
エチル・ケトンと共に第1表に示す割合で配合し混合し
た。
Back 1■Using koshiki with an average particle size of 10 μm as the hard particles of the composite layer,
5US31 with a particle diameter of 30 μm as a physical property adjusting particle
Using 6 and 5 US410 particles (which have a higher melting point than the self-fusing alloy that is the matrix metal described later), acrylic resin using these particles as an organic binder and methyl chloride as an organic solvent are used.
It was blended and mixed with ethyl ketone in the proportions shown in Table 1.

第1表 耐蝕耐摩耗材料の配合比(重量比〉種類 WC
5US410 5IJS316 7クリル■ メ+& 
工’r lyケ)7A100003        6 B752503        6 C6535036 D   50  50    0     3    
   6E750253        6 F650353        6 G500503         に のスラリーを加温してメチル・エチル・ケトンを蒸発乾
固させ、35〜80メツシユに粉砕分級した。この造粒
粉を静水圧装置を用いて基材表面に100 xloo 
xlotに100100O/cn2で成形した。この成
形体にN;・B・Slの自溶性合金を接触するように配
置し、真空炉に挿入した。これを1o−21orr真空
雰囲気で昇温し、アクリル樹脂を400°Cで蒸発分解
させた後、1080℃で20分間保持し、前記自溶性合
金を成形体に浸透させて複合層を形成し、かつ基材に接
合させた。
Table 1 Compounding ratio of corrosion-resistant and wear-resistant materials (weight ratio) Type WC
5US410 5IJS316 7krill■ Me+&
7A100003 6 B752503 6 C6535036 D 50 50 0 3
The slurry of 6E750253 6 F650353 6 G500503 was heated to evaporate methyl ethyl ketone to dryness, and then pulverized and classified into 35 to 80 meshes. This granulated powder was applied to the surface of the base material at a rate of 100 x loo using a hydrostatic pressure device.
It was molded in xlot at 100100O/cn2. A self-fusing alloy of N;.B.Sl was placed in contact with this molded body, and the molded body was inserted into a vacuum furnace. This is heated in a vacuum atmosphere of 10-21 orr to evaporate and decompose the acrylic resin at 400°C, and then held at 1080°C for 20 minutes to infiltrate the self-fusing alloy into the molded body to form a composite layer. and was bonded to the base material.

この焼結体について大越式迅速摩耗試験(相手材5KD
11 、HRC58、摩擦速度0.8n/sec 、摩
擦比i1?600 m ) 、硬さ、線膨張率、曲げ強
度、耐蝕性テストを行った。この結果を第2表に示す。
This sintered body was subjected to the Okoshi type rapid abrasion test (opposite material 5KD).
11, HRC58, friction speed 0.8 n/sec, friction ratio i1?600 m), hardness, coefficient of linear expansion, bending strength, and corrosion resistance tests. The results are shown in Table 2.

第2表 機械的性質 種類 比摩耗量 硬さ 線膜vjL率 曲げ強度nn+
3/kq、nm  HRC1/℃kc+f/mm2A 
 3.25x 10−’  64   8.0   9
0.5B  3.35x10 ’  5g    9.
1  103.5C4,20x 10−’  52  
 9.8  120.4D  1.80x10 ’  
48  10.5  135.OE  3.80x 1
0−’  57  11.1  101.5F  5.
05x 10−’  50  12.0  115.4
G  3.50x 10−845  13.4  12
0.0結果ニ示すように、SUS添加(B、C−D、E
、F= G)の場合、無添加の場合と比較すると耐摩耗
性は次第に低下するか、線膨張率、曲げ強度共に大きく
なることか分る。なお、第1表および第2表の種類り、
Gの場合でも、HRCは48および45を示しており、
一般の材料と比較すると十分高い硬度すなわち耐摩耗性
を有している。
Table 2 Mechanical property type Specific wear amount Hardness Linear film vjL ratio Bending strength nn+
3/kq, nm HRC1/℃kc+f/mm2A
3.25x 10-' 64 8.0 9
0.5B 3.35x10' 5g 9.
1 103.5C4, 20x 10-' 52
9.8 120.4D 1.80x10'
48 10.5 135. OE 3.80x 1
0-' 57 11.1 101.5F 5.
05x 10-' 50 12.0 115.4
G 3.50x 10-845 13.4 12
0.0 As shown in the result, SUS addition (B, CD, E
, F=G), it can be seen that the wear resistance gradually decreases or both the coefficient of linear expansion and bending strength increase when compared to the case without additives. In addition, the types in Tables 1 and 2,
Even in the case of G, the HRC shows 48 and 45,
It has sufficiently high hardness, that is, wear resistance, compared to general materials.

K嵐■ユ 複合層の硬質粒子として平均粒径10μmの一〇を用い
、物性調整粒子として粒径20μmアンダーの5US3
16粒子を用い、これらを有機バインダとするアクリル
樹脂と有機溶剤とするメチル・エチル・ゲトンと共に、
重量比で65: 35: 3 : 6の割合で配合し混
合した。
10 with an average particle size of 10 μm was used as the hard particles of the K Arashi ■ Yu composite layer, and 5US3 with a particle size of under 20 μm was used as the physical property adjustment particles.
Using 16 particles, together with acrylic resin using these as an organic binder and methyl ethyl getone as an organic solvent,
They were blended and mixed in a weight ratio of 65:35:3:6.

このスラリーを加温してメチル・エチル・ゲトンを蒸発
乾固させ、35〜80メツシユに粉砕分級した。この造
粒粉を第1図に示すようにプラスチックス成形機のスク
リュー形状に加工した基材10 (5CH435)表面
に、静水圧装置を用いて1!500kgf/cn+2で
成形した。この成形体20を第2図に示すようにスクリ
ュー形状の基材表面にIIIIIの厚さに機械加工した
。前記加工しな成形体にNi基合金(N+: B : 
Si:Fe=Bal  : 2 : 2.5 : 5重
量比)を接触させた状態で真空炉に挿入し、以下の条件
で焼結した。すなわち、焼結条件は、1O−2Torr
真空雰囲気で昇温し、400″Cでアクリル樹脂を分解
させた後、1080°Cで30分保持する条件とした。
This slurry was heated to evaporate the methyl ethyl getone to dryness, and then pulverized and classified into 35 to 80 meshes. As shown in FIG. 1, this granulated powder was molded onto the surface of a screw-shaped base material 10 (5CH435) of a plastics molding machine using a hydrostatic pressure device at a pressure of 1500 kgf/cn+2. As shown in FIG. 2, this molded body 20 was machined onto the surface of a screw-shaped base material to a thickness of III. Ni-based alloy (N+: B:
Si:Fe=Bal: 2:2.5:5 weight ratio) was inserted into a vacuum furnace in a state in which they were in contact with each other, and sintered under the following conditions. That is, the sintering conditions are 1O-2Torr
The temperature was raised in a vacuum atmosphere to decompose the acrylic resin at 400''C, and then held at 1080°C for 30 minutes.

この結果、従来技術である物性調整粒子を混合しない場
合は、実施例1に示したように線膨張率か8.0 1/
”Cと小さく 、5CH435のような線膨張率が11
.5 1/”Cと大きな基材に被覆する場合は、複合層
に割れか生じたりしたが、本発明によれば割れも生じる
ことがなく、良好な複合層が得られた。
As a result, in the case of not mixing physical property adjusting particles, which is the conventional technique, as shown in Example 1, the linear expansion coefficient was 8.0 1/
"C is small, and the coefficient of linear expansion is 11 like 5CH435.
.. When coating a substrate as large as 5 1/''C, cracks occurred in the composite layer, but according to the present invention, no cracks occurred and a good composite layer was obtained.

実施例3 複合層の硬質粒子として平均粒径10μmのWCを用い
、物性調整粒子として粒径30μmアンダーのCo基合
金、Ni基合金(成分を第3表に示す)粒子を用い、こ
れらを有機バインダとするアクリル樹脂と有機溶剤とす
るメチル・エチル・ゲトンと共に第4表に示す割合で配
合し混合した。
Example 3 WC with an average particle size of 10 μm was used as the hard particles of the composite layer, and Co-based alloy and Ni-based alloy (components are shown in Table 3) particles with a particle size of less than 30 μm were used as the physical property adjusting particles. An acrylic resin as a binder and methyl ethyl getone as an organic solvent were mixed together in the proportions shown in Table 4.

第3表 C01Ni基合金の成分(重量%)成分 材種   Cr Co1合金  :27〜28 Ni基合金  8.0〜15 Co基合金  2.0〜3.O Ni基合金    Ba CoI合*  4.0〜13 Ni基合金 CHn      N。Table 3: Composition (wt%) of C01Ni-based alloy Material type Cr Co1 alloy: 27-28 Ni-based alloy 8.0-15 Co-based alloy 2.0-3. O Ni-based alloy Ba CoI match* 4.0~13 Ni-based alloy CHn    N.

1.0〜1.5   ≧ 11.0〜1.5≧0.1 
        20〜30co    Fe    
    5 Bat  2.0〜3.0  1.0〜1.52.0〜
4.0 第4表 配合比(重量比) 複合層材I   WCCo11*  Ni基合金 アク
リルIl脂 メチルエチルケトンCoi台金!65  
 35    −    3        6〜1基
合金茶 65   −    35    3    
     にのスラリーを実施例1と同様に造粒し、静
水圧装置を用いて基材表面(SUS420 J2)に1
00 xloo x15tに1500kgf/cm2で
成形しな、この成形体にNi−B−3iの自溶性合金を
接触するように配置し、真空炉に挿入した。
1.0-1.5≧11.0-1.5≧0.1
20~30co Fe
5 Bat 2.0~3.0 1.0~1.52.0~
4.0 Table 4 Mixing ratio (weight ratio) Composite layer material I WCCo11* Ni-based alloy Acrylic Il fat Methyl ethyl ketone Coi base metal! 65
35-3 6-1 base alloy tea 65-35 3
The slurry of
A self-fusing alloy of Ni-B-3i was placed in contact with this molded body, and the molded body was inserted into a vacuum furnace.

これを1O−2Torr真空雰囲気で昇温し、アクリル
樹脂を400℃で蒸発分解させた後、1150℃で60
分間保持し、前記自溶性合金を成形体に浸透させて複合
層を形成し、かつ基材に接合させた。
This was heated in a vacuum atmosphere of 10-2 Torr to evaporate and decompose the acrylic resin at 400°C, and then heated to 1150°C for 60°C.
The self-fusing alloy was held for a minute to infiltrate the compact to form a composite layer and bond it to the substrate.

これらの焼結体について実施例1と同様にして摩耗試験
、硬さ測定を行った後、複合層のみを10x 10x 
80の形状に加工し、シャルピー衝撃試験を行った。こ
の結果を第5表に示す。
After performing wear tests and hardness measurements on these sintered bodies in the same manner as in Example 1, only the composite layer was
It was processed into a size 80 and subjected to a Charpy impact test. The results are shown in Table 5.

第5表 機械的性質 複合層 比摩耗量  硬さ 衝撃値 材種  IIE’ /kg、1m  HRCkgf/c
n+2Coi合金系  4.3  xlo  ’   
 55    0.9Nii合金系  3.3  xl
o−9600,6IllC!合II    3.25X
 10−’    64    0.3この結果、比摩
耗量はACのみの複合層と同程度であるが、衝撃値は2
〜3倍に向上した。
Table 5 Mechanical properties Composite layer Specific wear Hardness Impact value grade IIE' /kg, 1m HRCkgf/c
n+2 Coi alloy system 4.3 xlo'
55 0.9Nii alloy system 3.3 xl
o-9600,6IllC! Combined II 3.25X
10-' 64 0.3 As a result, the specific wear amount is the same as that of the AC-only composite layer, but the impact value is 2
~3 times improved.

この組繊を観察すると、マトリックスであるNi・B−
3iの自溶性合金のBが、Co、Ni基合金表面に浸硼
したため、Ni自溶合全中の脆弱層であるNi、 Bの
金属間化合物の生成が減少し、この結果複合層の靭性か
向上したことか分る。
Observing this composite fiber, we can see that the matrix Ni・B−
Since B of the self-fusing alloy of 3i infiltrated the surface of the Co and Ni-based alloy, the formation of the intermetallic compound of Ni and B, which is a weak layer in the Ni self-fusing alloy, was reduced, and as a result, the toughness of the composite layer was reduced. I can see if it has improved.

【図面の簡単な説明】[Brief explanation of drawings]

第1図は基材の表面に硬質粒子と金属粒子との混合体の
層を設けた図、第2図は第1図の混合体層を所定厚さに
機械加工した状態を示す図である。 10・・・スクリュー   20・・・成形体特許出願
人   東芝機械株式会社− 出願人代理人  弁理士 浜田樟雄 \、2
Figure 1 is a diagram showing a layer of a mixture of hard particles and metal particles provided on the surface of a base material, and Figure 2 is a diagram showing a state where the mixture layer of Figure 1 has been machined to a predetermined thickness. . 10...Screw 20...Molded object patent applicant Toshiba Machine Co., Ltd. - Applicant's agent Patent attorney Hamada Kusuo\,2

Claims (6)

【特許請求の範囲】[Claims] (1)複合層の硬質粒子として炭化物、硼化物、窒化物
の内少くとも1種以上と、複合層の物性調整粒子として
金属粒子と、複合層のマトリックス金属としてFe基合
金、Ni基合金、Co基合金の内少くとも1種以上とを
含有する複合層を基材表面に接合させたことを特徴とす
る高強度耐蝕耐摩耗性材料。
(1) At least one or more of carbides, borides, and nitrides as hard particles of the composite layer, metal particles as physical property adjusting particles of the composite layer, Fe-based alloy, Ni-based alloy as the matrix metal of the composite layer, A high-strength corrosion-resistant and wear-resistant material characterized by having a composite layer containing at least one type of Co-based alloy bonded to the surface of a base material.
(2)物性調整粒子が、Fe基合金、Ni基合金、Co
基合金、Cu合金の内少くとも1種以上からなる請求項
1記載の高強度耐蝕耐摩耗性材料。
(2) The physical property adjusting particles are Fe-based alloy, Ni-based alloy, Co
The high-strength corrosion-resistant and wear-resistant material according to claim 1, comprising at least one of a base alloy and a Cu alloy.
(3)物性調整粒子が、複合層のマトリックス金属より
融点の高い合金粒子である請求項1記載の高強度耐蝕耐
摩耗性材料。
(3) The high-strength corrosion-resistant and wear-resistant material according to claim 1, wherein the physical property adjusting particles are alloy particles having a higher melting point than the matrix metal of the composite layer.
(4)複合層の硬質粒子として炭化物、硼化物、窒化物
の内少くとも1種以上と、複合層の物性調整粒子として
金属粒子とからなる混合粒子を基材表面形状に固定し、
更に前記混合粒子に接触するよう複合層のマトリックス
金属を配置し(複合層のマトリックス金属としてFe基
合金、Ni基合金、Co基合金の内少くとも1種以上を
含有する)、加熱源で加熱し、マトリックス金属を溶融
させ、混合粒子の間隙に浸透させて複合層を形成すると
共に基材表面に拡散接合させることを特徴とする高強度
耐蝕耐摩耗性材料の製造方法。
(4) fixing mixed particles consisting of at least one or more of carbides, borides, and nitrides as hard particles of the composite layer and metal particles as physical property adjusting particles of the composite layer to the surface shape of the base material;
Furthermore, a matrix metal of the composite layer is arranged so as to be in contact with the mixed particles (the matrix metal of the composite layer contains at least one of Fe-based alloy, Ni-based alloy, and Co-based alloy), and heated with a heating source. A method for producing a high-strength, corrosion-resistant and wear-resistant material, characterized by melting a matrix metal, allowing it to penetrate into the gaps between mixed particles to form a composite layer, and diffusion bonding to the surface of a base material.
(5)物性調整粒子が、Fe基合金、Ni基合金、Co
基合金、Cu合金の内少くとも1種以上からなる請求項
4記載の高強度耐蝕耐摩耗性材料の製造方法。
(5) The physical property adjusting particles are Fe-based alloy, Ni-based alloy, Co
The method for producing a high-strength corrosion-resistant and wear-resistant material according to claim 4, which comprises at least one of a base alloy and a Cu alloy.
(6)物性調整粒子を、複合層のマトリックス金属より
融点の高い合金粒子とする請求項4記載の高強度耐蝕耐
摩耗性材料の製造方法。
(6) The method for producing a high-strength corrosion-resistant and wear-resistant material according to claim 4, wherein the physical property adjusting particles are alloy particles having a higher melting point than the matrix metal of the composite layer.
JP15532190A 1990-06-15 1990-06-15 Corrosion and wear resistant material having high strength and its production Pending JPH0448083A (en)