JPH0451940B2 - - Google Patents

Info

Publication number
JPH0451940B2
JPH0451940B2 JP62076025A JP7602587A JPH0451940B2 JP H0451940 B2 JPH0451940 B2 JP H0451940B2 JP 62076025 A JP62076025 A JP 62076025A JP 7602587 A JP7602587 A JP 7602587A JP H0451940 B2 JPH0451940 B2 JP H0451940B2
Authority
JP
Japan
Prior art keywords
weight
polyolefin
sealing material
thin battery
ethylene
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Lifetime
Application number
JP62076025A
Other languages
Japanese (ja)
Other versions
JPS63244551A (en
Inventor
Hidetomo Ashitaka
Tooru Takahashi
Ryuichi Shimizu
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Ube Corp
Original Assignee
Ube Industries Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Ube Industries Ltd filed Critical Ube Industries Ltd
Priority to JP62076025A priority Critical patent/JPS63244551A/en
Publication of JPS63244551A publication Critical patent/JPS63244551A/en
Publication of JPH0451940B2 publication Critical patent/JPH0451940B2/ja
Granted legal-status Critical Current

Description

【発明の詳細な説明】 [産業上の技術分野] 本発明は、正負両極の集電体を兼ねる外装板の
周縁部を、特に密着性およびベンデイング特性が
優れた封口材であり、耐ヒートシヨツク性をも有
する封口材で密封することを特徴とする長期保存
安定性の優れた薄形電池に関する。 [発明の技術的背景とその問題点] 最近、電子機器の小形化、薄膜化が進展するに
伴つて、それらの電源としての電池においても、
小形化、薄膜化が強く求められている。特に、メ
モリーカード、ICカードなどのカード型電子機
器に適した、いわゆる、シート状電池やペーパ
ー・バツテリーなどが実用化されている。これら
の電池の薄型化においては、電池の密封方法が大
きな技術的課題となつてきている。 これらの薄形電池は、集電体を兼ねる正負両極
の平板状外装板の周縁部を、熱接着性樹脂で密封
する構造が提案されている。 この熱接着性樹脂としては、次のような特性が
要求されている。すなわち、正負極の厚みが小さ
くなるにつれて、両極間の絶縁が充分保持され、
かつ、密着性の良好で電解液の液もれなどがな
く、長期保存性の優れた封口材が必要となる。さ
らに、高エネルギー密度の観点から、負極活物質
としてリチウムを、そして、有機溶媒に無機塩を
溶解した非水電解液を電解質とした、いわゆる、
非水電解液リチウム電池系の薄膜電池の開発が盛
んに行なわれている。その場合、さらに、封口材
の特性として、リチウムと反応しやすい水分が外
部から吸収しにくく、また、有機電解液に化学的
に安定で、膨潤などが起こらない特性が必要であ
る。 これらの特性を満足する熱接着性樹脂として
は、ポリオレフイン系樹脂、フツ素系樹脂、およ
び、それらの変性物が種々提案されており、例え
ば、特開昭49−128232号、同60−14753号、同60
−148050号、同60−160559号、同60−185359号、
同60−185360号、同60−220553号、同61−68860
号、同61−185867号、同61−74256号、同61−
176054号、同61−185867号などが開示されてい
る。 これらの方法は、ポリオレフイン樹脂が無極性
であるため、優れた化学的、電気的性質を有して
いることを利用したものである。しかし、ポリオ
レフイン樹脂は、接着性に乏しく、そのため、上
記の従来技術では、エチレンと酢酸ビニルとの共
重合体、アイオノマー樹脂あるいは不飽和カルボ
ン酸をグラフトしたポリオレフイン樹脂などの変
性体を用いることを提案している。 しかしながら、これらの変性体は必ずしも前記
の封口材としての要求特性を満足させるほど充分
な接着性を有しているとは言えず、これらを封口
材として用いた電池は長期信頼性に問題があり、
さらに優れた接着性、ベンデイング特性、耐ヒー
トシヨツク性を有する封口材が求められている。 そこで、ポリオレフイン樹脂に接着性を付与す
るために、種々の改良方法が提案されている。そ
の一つとして、ポリオレフイン樹脂をγ−メタア
クリロイルオキシプロピルトリメトキシシラン、
グリシジルメタクリレートなどから選ばれた一種
の変性剤と有機過酸化物とで変性してポリオレフ
イン樹脂の接着性を改良する方法が提案されてい
る。しかしながら、この方法によつて得られる変
性ポリオレフインの接着性改良は未だ満足すべき
ものとは言えない。 また、薄形電池では、ベンデイング特性が要求
され、封口材もベンデイングテストの後、外装板
との密着性が保持され、また、クラツクなどが生
じないことが必要である。 前記の従来方法によつて得られる変性ポリオレ
フイン樹脂は、これらの特性が不充分である。 従つて、本発明の目的は、従来の薄膜電池の欠
点を改良した、特に密着性およびベンデイング特
性が優れた封口材であり、耐ヒートシヨツク性を
も有する封口材を用いた長期安定性の優れた薄膜
電池を提供することにある。 [問題を解決するための手段] 本発明は、 集電体を兼ねた対向した一対の金属薄板からな
る外装板の内部に、正極と負極との中間に電解質
を含むセパレータあるいは固体電解質の隔膜を形
成し、外装板の周縁を封口材で密封した薄形電池
であつて、前記封口材として、下記(a)乃至(d)の各
成分のうち少なくとも2成分を含有しており、各
成分の配合割合は、ポリマー重量中(a)が10〜100
重量%、(b)が0〜90重量%、(c)が0〜90重量%で
あり、全組成物重量中(d)が5〜50重量%である接
着性ポリオレフイン組成物を用いることを特徴と
する薄形電池。 (a) ポリオレフインとアルケニルコハク酸類また
は式CR1R2=CR3−CO−R4(式中、R1,R2及
びR3はHまたは炭素数1〜10のアルキル基で
あり、R4はベンゾトリアゾール、フタルイミ
ド、オルソスルホベンゾイミド、1,8−ナフ
タルイミド、コハク酸イミド、ラクタム類及び
これらの誘導体からHを除いた残基である。)
で表わされる不飽和化合物とをグラフト反応し
て得られる変性ポリオレフイン。 (b) 未変性のポリオレフイン (c) エラストマー (d) 炭酸カルシウム を提供することにより、前記目的を達成したもの
である。 この発明の薄形電池に用いられる封口材組成物
の各成分について詳述する。 本発明においてはポリオレフインとアルケニル
コハク酸類または式CR1R2=CR3−CO−R4(式
中、R1,R2及びR3はHまたは炭素数1〜10のア
ルキル基であり、R4はベンゾトリアゾール、フ
タルイミド、オルソスルホベンゾイミド、1,8
−ナフタルイミド、コハク酸イミド、ラクタム類
及びこれらの誘導体からHを除いた残基である。)
で表わされる不飽和化合物とをグラフト反応して
得られる変性ポリオレフイン(a)を使用する。 本発明において使用されるポリオレフインとし
ては、エチレン、プロピレン、ブテン−1、ヘキ
セン−1、デセン−1,4−メチルブテン−1,
4−メチルペンテン−1などのエチレン系オレフ
インの単独重合体および共重合体、そしてこれら
のオレフインと非共役ジエン(例えば、1,4−
ヘキサジエン、ペンタジエン、ジシクロペンタジ
エン、メチルテトラヒドロインデン、メチレンノ
ルボルネン、エチリデンノルボルネン)からなる
共重合体を挙げることができる。これらのうちで
もポリプロピレンが特に好ましい。 また本発明で使用されるポリオレフインには、
エチレン・プロピレンゴム、ブチルゴム、エチレ
ン・ブタジエンゴム等のゴム類、エチレン/アク
リル酸、エチレン/エチルアクリレート、エチレ
ン/酢酸ビニル、アイオノマーもまた含まれる。
これらのポリオレフインは単独で使用してもよ
く、あるいは二種類以上併用することもできる。 本発明においてポリオレフインの変性に使用さ
れる不飽和化合物としては、ドデセニルコハク酸
無水物、オクタデセニルコハク酸無水物、4−メ
タクリロキシエチルトリメリト酸無水物等のアル
ケニルカルボン酸無水物、及びその誘導体、上記
酸無水物に対応するジカルボン酸、そのモノエス
テル、金属塩等が挙げられる。 さらに本発明において、不飽和化合物として
は、式CR1R2=CR3−CO−R4(式中、R1,R2及
びR3はHまたはアルキル基であり、R4はベンゾ
トリアゾール、フタルイミド、オルソスルホベン
ゾイミド、1,8−ナフタルイミド、コハク酸イ
ミド、ラクタム類等及びその誘導体からHを除い
た残基である。)で表わされる化合物を使用する
ことができる。具体的には、1−アクリロイルベ
ンゾトリアゾール、1−アクリロイルフタルイミ
ド、1−アクリロイルスルホベンゾイミド、1−
アクリロイルナフタルイミド、メタアクリロイル
ベンゾトリアゾール等、及びこれらの誘導体が挙
げられる。 また、本発明においては、上記不飽和化合物と
他の不飽和単量体との併用も可能であり、他の不
飽和単量体としては、α,β不飽和カルボン酸、
それらのモノエステルおよび無水物等が挙げられ
る。さらに具体的に例示するならば、アクリル
酸、メタクリル酸、マレイン酸、マレイン酸モノ
メチルエステル、無水マレイン酸、イタコン酸、
イタコン酸モノメチルエステル、無水イタコン
酸、フマル酸、及びこれらの誘導体、並びにこれ
らの酸の金属塩等を挙げることができる。また循
環式カルボン酸、さらに具体的には、エンド−ビ
シクロ(2,2,1)−5−ヘプテン−2,3−
カルボン酸無水物、シス−4−シクロヘキセン−
1,2−カルボン酸無水物、及びこれらの誘導
体、並びにこれらの酸の金属塩等を用いることが
できる。あるいは、アクリル酸エステル、エポキ
シ基含有化合物、例えばグリシジルメタクリレー
ト等も使用可能である。 本発明に使用される不飽和化合物の添加量は、
ポリオレフイン100重量部に対して、好ましくは
0.01〜5.0重量部であり、特に好ましくは0.01〜
2.0重量部である。 ポリオレフインと前記不飽和化合物とのグラフ
ト反応は、通常ターシヤリーブチルハイドロパー
オキサイド、ジターシヤリーブチルパーオキサイ
ド、ジクミルパーオキサイド、ベンゾイルパーオ
キサイド等の有機過酸化物の存在下の加熱して行
なわれる。有機過酸化物の添加量は、ポリオレフ
イン100重量部に対して0.01〜5.0重量部、特に
0.01〜1.0重量部が好ましい。 前記不飽和化合物は、ポリマー重量〔(a)+(b)+
(c)〕中、0.01〜2.0重量%の割合で含まれるのが
好ましい。 また変性ポリオレフインを製造する際に、酸化
マグネシウム、水酸化アルミニウム、水酸化マグ
ネシウム、酸化アンチモン等を同時に添加して酸
成分を金属化することも出来るし、充填剤を添加
することも出来る。一般には未変性ポリオレフイ
ンへ充填剤を添加しておく方が好ましい。 変性ポリオレフインは通常ペレツトの形状に成
形される。 また、この発明で用いる未変性ポリオレフイン
(b)としては、前記のポリオレフインが挙げられ
る。変性ポリオレフインを得るために用いたもの
と同じ種類のものが好適に使用される。 未変性のポリオレフインには、従来公知の添加
剤(酸化防止剤、紫外線吸収剤など)が配合され
ていてもよい。粉末状無機物質、変性ポリオレフ
インは、それぞれ未変性のポリオレフインのマス
ターバツチにして使用してもよい。 本発明に使用されるエラストマー(c)として、変
性、未変性ポリオレフイン重合体よりも常温にお
ける引張弾性率(ASTMD−882−73)が低い重
合体が用いられる。 具体的には、各種ポリエチレン、エチレン/プ
ロピレン、エチレン/プロピレン/ジエン、エチ
レン/ブテン、スチレン/ブタジエン、エチレ
ン/アクリル酸、エチレン/エチルアクリレー
ト、アイオノマー、エチレン/酢ビ等の共重合
体、液状ゴム類、及びこれらに不飽和酸、酸のエ
ステル、金属塩、イミド、アミド等の誘導体や不
飽和シラン化合物を付加した変性物、部分架橋物
も使用される。変性結晶性ポリプロピレンに対し
てエチレン/プロピレン(ジエン)ラバーまたは
その変性物が好ましい。 また、これらの組成物において相溶性のあるポ
リアミド類、例えばナイロン6、ナイロン12、ポ
リエステルアミド、ポリエーテルアミド、ポリエ
ステルエーテルアミド等を変性ポリオレフインと
エラストマーとの総量に対して重量比で1:1を
こえない範囲で使用することができる。 本発明で用いる炭酸カルシウム(重質、軽質)
(d)は、平均粒径が0.05〜10μ、特に0.5〜5μ、比表
面積が0.1〜100m2/g、特に1〜30m2/gの粉末
状のものが好ましい。炭酸カルシウムは表面処理
されていないものが好ましい。 また炭酸カルシウム以外に、タルク、マイカ、
酸化ケイ素等の無機物質や、ケイ素の炭酸化物、
水酸化物、酸化物等も添加出来る。 本発明の接着性ポリオレフイン組成物は、前記
各成分の配合割合が、ポリマー重量中(a):変性ポ
リオレフイン10〜100重量%、(b):未変性のポリ
オレフイン0〜90重量%、(c):エラストマー0〜
90重量%(好ましくは5〜60重量%)、全組成物
重量中(d):炭酸カルシウム5〜50重量%となるよ
うに混合することによつて得ることができる。各
成分の割合が前記範囲外であると、得られる組成
物の接着性が低下する。 (a)の割合が10重量%より少ないと接着性が低下
し、(b)の割合が90重量%より多いと接着性が低下
し、(c)の割合が90重量%より多いと接着性が低下
する。(b)の割合が5重量%より少ないと接着性が
低下し、熱変化に対する変形が大きくなる。ま
た、50重量%より多いと脆くなる欠点が生じる。 本発明の接着性ポリオレフイン組成物は、混合
時に、各種添加剤、例えば耐候(熱)性安定剤、
成形助剤などを添加してもよい。最も簡便な混合
操作は、前記各成分を約180〜350℃、特に220〜
270℃の温度で1〜10分間程度押出機内で溶融混
合することである。押出機としては一軸または二
軸押出機やFCMなどのコンテイニユアスミキサ
ーが挙げられる。溶融混合の際に、脱気操作(ベ
ント)を行なうと本発明の効果は一層向上する。
これは、粉末状無機物質の表面に付着水分がある
ためである。 この発明における組成物は、(a)乃至(d)の各成分
を前記特定の割合で混合することによつて、従来
公知のポリオレフイン樹脂系の接着剤と比較し
て、金属薄板に対して大きな接着強度を有してお
り、封口材としてきわめて優れた特性を発揮して
長期保存特性の良好な薄形電池を得ることができ
る。組成物中の各成分の配合割合が前記範囲外で
あると、接着性、ベンデイング特性、耐ヒートシ
ヨツク性を有する組成物を得ることがきない。 上記の組成物を封口材として用いて、薄形電池
を得る方法は特に限定されるものではなく、例え
ば、シートあるいはフイルム化し、それを、窓枠
シート部材として、内部に正極、電解質隔膜およ
び負極を積層した一対の金属薄板外装板の周縁部
に挟み、熱圧着することにより、密封性の優れた
薄形電池を得ることができる。また、前記シート
あるいはフイルムは、本発明の組成物を接着層と
し、中間部に未変性の樹脂からなる中間層を設け
た三層シート、三層フイルムとして使用すること
もできる。 [本発明の実施例] 次に実施例および比較例を示す。 以下の記載において、部は重量部を示し、メル
トフローレイト(MFR)はASTMD1238に従つ
て測定した。また、長期保存安定性は製造後60日
間放置した後、200μAの定電流放電試験を行なつ
た。 ベンデイング特性試験はICカードの曲げ強度
測定法(DP7816/1)に準じて行なつた。 即ち第1図に示すたわみ量0〜3mmになるよう
に可動部を左右に繰返し移動させた。 なお、実施例、比較例の接着剤組成物はまとめ
て第1表に示す。 (使用材料) ポリオレフイン 1 ポリプロピレン エチレン−プロピレンブロツク共重合体:ポリ
プロピレン(A)(宇部興産(株)製 J701H) 2 ポリエチレン 低密度ポリエチレン:ポリエチレン(B)(宇
部興産(株)製 F222) 3 エチレン−プロピレンラバー エチレン/プロピレン/エチリデンノルボルネ
ンターポリマー:エチレンプロピレンラバー(c)
(日本合成ゴム(株)製 EP−57P) 有機過酸化物 t−ブチルハイドロパーオキサイド 不飽和化合物 1 アルケニルコハク酸無水物(炭素数15)(三
洋化成(株)製 DSA) 〔実施例 1〕 (封口材シートの作成法) ポリプロピレン(A)〔引張弾性率:14200Kg/
cm2〕100重量部に対して、アルケニルコハク酸無
水物2.0重量部及びt−ブチルハイドロパーオキ
サイド0.5重量部をドライブレンド後、内径30mm、
L/D=17の二軸押出機を用いて250℃、吐出量
2Kg/時で溶融混練してペレツトにした。このペ
レツトを減圧下、加熱乾燥し、変性ポリオレフイ
ン(1)を得た。 変性ポリオレフイン(1)90重量部と炭酸カルシウ
ム〔重質、平均粒径2.1μ、比表面積10.5m2/gの
粉末状〕10重量部を、ブレンダーで混合した後、
50mmφベント式一軸押出機にて250℃で2分間溶
融混練して、2mmφ×3mm程度の接着性ポリオレ
フイン組成物のペレツトを得た。これより接着性
ポリオレフインシートを作成した。 このシートから、打抜き刃で外形40×40mmで、
幅4mmの環状封口材シートを作成した。 (正極合剤の作成法) 二酸化マンガン332.9mg、アセチレンブラツク
62.4mgの混合物に、メトキシポリエチレングリコ
ールモノアクリレート(新中村化学製AM−
90G)31.4mg、ポリエチレングリコールジメタク
リレート(新中村化学製9G)10.7mg、ジメトキ
シポリエチレングリコール(旭電化製LX−521)
に過塩素酸リチウムを溶解させた(濃度0.75m
mol/)溶液62.8mg、および、ベンゾイルパー
オキサイド0.067mgをさらに混合し、正極合剤と
した。 (正極の作成法) 負極集電体兼外装板として、寸法が40×40×
0.05mmのステンレス箔に、上記の正極合剤を28×
28mmの大きさに均一に塗布した。これを加圧成形
し、100℃、3時間加熱して正極板(300μmの厚
み)と外装板からなる正極積層体Aを作成した。 (負極および電解質隔膜の作成法) 負極集電体兼外装板として、寸法が40×40×
0.05mmのステンレス箔に、寸法が26×26×0.07mm
のリチウム箔を圧着した。 電解質用の組成物として、AM−90Gを18.4mg、
9Gを6.0mg、過塩素酸リチウムをLX−521に溶解
した溶液(濃度0.75 mol/)を25.6mg、およ
び、光増感剤として2,2−ジメトキシアセトフ
エノン0.1mgの混合液を準備した。この電解質溶
液を8μを前記リチウム金属円板に塗布し、
250Wの超高圧水銀灯を用い、5mW/cmの照度で
3分間照射して厚み50μmの硬化フイルムを形成
させ、集電体兼外装板、負極、および電解質隔膜
の積層体Bを作成した。 (電池の組み立て) 上記の積層体AおよびBを積層し、外装板周縁
部に前記の環状封口体シートを挟み、加熱圧着
(180℃、3Kg/cm2、3分間)して、薄形電池を
組み立てた。 以下、電池放電試験の結果を第2図に示す。 なお、電池について、ベンデイングテスト
5000回後も、封口部、電気特性に異常は認められ
なかつた。 〔実施例 2〕 変性ポリオレフイン(1)とポリプロピレン(A)
と炭酸カルシウムとの併用系で、これらの溶融混
練物を用いて、実施例1と同様にして薄形電池
を組み立てた。 なお、ベンデイングテスト結果は実施例1と同
様であつた。 〔実施例 3〕 実施例2においてポリプロピレン(A)の一部
に代えてエチレンプロピレンラバー(C)〔EPR
(C)〕を用いた以外は、実施例2と同様にして薄
形電池を組み立てた。 なお、ベンデイングテスト結果は実施例1と同
様であつた。 [実施例 4] 実施例3においてEPR(C)に代えて未変性の
ポリエチレン(B)〔PE(B)〕を用いた以外は、
実施例3と同様にして薄形電池を組み立てた。 なお、ベンデイングテスト結果は実施例1と同
様であつた。 [比較例 1] ポリプロピレン(A)と炭酸カルシウムとの混
練物を用いた以外は、実施例1と同様にして薄形
電池を組み立てた。 なお、ベンデイングテストを行なつたところ、
1000回で封口部に剥離が認められた。 〔比較例 2〕 変性ポリプロピレン(1)とエチレンプロピレンラ
バー(C)との混練物を用いた以外は、実施例1
と同様にして薄形電池を組み立てた。 なお、ベンデイングテスト結果は比較例1と同
様であつた。 【表】
Detailed Description of the Invention [Industrial Technical Field] The present invention is a sealing material that has particularly excellent adhesion and bending properties, and is heat shock resistant, for sealing the peripheral edge of an exterior plate that also serves as a current collector for both positive and negative electrodes. The present invention relates to a thin battery with excellent long-term storage stability, which is characterized by being sealed with a sealing material that also has properties. [Technical background of the invention and its problems] Recently, as electronic devices have become smaller and thinner, batteries as a power source for these devices have also become smaller and thinner.
There is a strong demand for smaller size and thinner film. In particular, so-called sheet batteries and paper batteries, which are suitable for card-type electronic devices such as memory cards and IC cards, have been put into practical use. In order to make these batteries thinner, the method of sealing the batteries has become a major technical issue. For these thin batteries, a structure has been proposed in which the periphery of a flat exterior plate with both positive and negative electrodes, which also serves as a current collector, is sealed with a thermoadhesive resin. This thermoadhesive resin is required to have the following properties. In other words, as the thickness of the positive and negative electrodes decreases, sufficient insulation is maintained between the two electrodes.
In addition, a sealing material with good adhesion, no electrolyte leakage, and excellent long-term storage stability is required. Furthermore, from the viewpoint of high energy density, so-called lithium is used as the negative electrode active material and a non-aqueous electrolyte in which an inorganic salt is dissolved in an organic solvent is used as the electrolyte.
Thin film batteries based on non-aqueous electrolyte lithium batteries are being actively developed. In this case, the sealing material must also have characteristics that make it difficult to absorb moisture that easily reacts with lithium from the outside, and that it is chemically stable to organic electrolytes and does not cause swelling. Various polyolefin resins, fluorocarbon resins, and modified products thereof have been proposed as heat-adhesive resins that satisfy these characteristics. , 60
-148050, 60-160559, 60-185359,
60-185360, 60-220553, 61-68860
No. 61-185867, No. 61-74256, No. 61-
No. 176054 and No. 61-185867 are disclosed. These methods utilize the fact that polyolefin resin is nonpolar and therefore has excellent chemical and electrical properties. However, polyolefin resins have poor adhesive properties, and therefore, the above-mentioned conventional technology proposes the use of modified products such as copolymers of ethylene and vinyl acetate, ionomer resins, or polyolefin resins grafted with unsaturated carboxylic acids. are doing. However, these modified products do not necessarily have sufficient adhesion to satisfy the above-mentioned required properties as a sealing material, and batteries using these as a sealing material have problems with long-term reliability. ,
There is a need for a sealing material that has even better adhesion, bending properties, and heat shock resistance. Therefore, various improvement methods have been proposed in order to impart adhesive properties to polyolefin resins. As one of them, γ-methacryloyloxypropyltrimethoxysilane, polyolefin resin,
A method has been proposed for improving the adhesiveness of polyolefin resins by modifying them with a type of modifier selected from glycidyl methacrylate and an organic peroxide. However, the improvement in adhesion of modified polyolefins obtained by this method is still not satisfactory. In addition, thin batteries require good bending properties, and the sealing material must maintain adhesion to the exterior plate after a bending test and must not cause cracks. Modified polyolefin resins obtained by the conventional methods described above are insufficient in these properties. Therefore, an object of the present invention is to provide a sealing material that improves the shortcomings of conventional thin film batteries, particularly in adhesion and bending properties, and provides excellent long-term stability using a sealing material that also has heat shock resistance. The purpose of the present invention is to provide a thin film battery with improved characteristics. [Means for solving the problem] The present invention includes a separator containing an electrolyte or a solid electrolyte diaphragm between a positive electrode and a negative electrode inside an exterior plate consisting of a pair of opposing thin metal plates that also serves as a current collector. The battery is a thin battery in which the periphery of the exterior plate is sealed with a sealing material, and the sealing material contains at least two of the following components (a) to (d). The blending ratio is 10 to 100 of (a) in the polymer weight.
% by weight, (b) is 0 to 90% by weight, (c) is 0 to 90% by weight, and (d) is 5 to 50% by weight based on the total composition weight. Features a thin battery. (a) Polyolefin and alkenylsuccinic acids or the formula CR 1 R 2 = CR 3 -CO-R 4 (wherein, R 1 , R 2 and R 3 are H or an alkyl group having 1 to 10 carbon atoms, and R 4 is a residue obtained by removing H from benzotriazole, phthalimide, orthosulfobenzimide, 1,8-naphthalimide, succinimide, lactams, and their derivatives.)
A modified polyolefin obtained by a graft reaction with an unsaturated compound represented by The above object has been achieved by providing (b) an unmodified polyolefin, (c) an elastomer, and (d) calcium carbonate. Each component of the encapsulant composition used in the thin battery of the present invention will be explained in detail. In the present invention, polyolefin and alkenylsuccinic acids or the formula CR 1 R 2 = CR 3 -CO-R 4 (wherein, R 1 , R 2 and R 3 are H or an alkyl group having 1 to 10 carbon atoms, and R 4 is benzotriazole, phthalimide, orthosulfobenzimide, 1,8
- It is a residue obtained by removing H from naphthalimide, succinimide, lactams, and derivatives thereof. )
A modified polyolefin (a) obtained by a graft reaction with an unsaturated compound represented by is used. The polyolefins used in the present invention include ethylene, propylene, butene-1, hexene-1, decene-1,4-methylbutene-1,
Homopolymers and copolymers of ethylene-based olefins such as 4-methylpentene-1, and combinations of these olefins with nonconjugated dienes (e.g., 1,4-
Examples include copolymers of hexadiene, pentadiene, dicyclopentadiene, methyltetrahydroindene, methylenenorbornene, ethylidenenorbornene. Among these, polypropylene is particularly preferred. In addition, the polyolefin used in the present invention includes
Also included are rubbers such as ethylene-propylene rubber, butyl rubber, ethylene-butadiene rubber, ethylene/acrylic acid, ethylene/ethyl acrylate, ethylene/vinyl acetate, and ionomers.
These polyolefins may be used alone or in combination of two or more. In the present invention, unsaturated compounds used for modifying polyolefins include alkenyl carboxylic anhydrides such as dodecenyl succinic anhydride, octadecenyl succinic anhydride, 4-methacryloxyethyl trimellitic anhydride, and the like. Examples include derivatives, dicarboxylic acids corresponding to the above acid anhydrides, monoesters thereof, and metal salts. Furthermore, in the present invention, the unsaturated compound has the formula CR 1 R 2 = CR 3 -CO-R 4 (wherein, R 1 , R 2 and R 3 are H or an alkyl group, and R 4 is benzotriazole, It is a residue obtained by removing H from phthalimide, orthosulfobenzimide, 1,8-naphthalimide, succinimide, lactams, etc. and their derivatives.) Compounds represented by the following can be used. Specifically, 1-acryloylbenzotriazole, 1-acryloyl phthalimide, 1-acryloylsulfobenzimide, 1-
Examples include acryloylnaphthalimide, methacryloylbenzotriazole, and derivatives thereof. In addition, in the present invention, it is also possible to use the above unsaturated compound in combination with other unsaturated monomers, and examples of other unsaturated monomers include α,β unsaturated carboxylic acids,
Examples include monoesters and anhydrides thereof. More specific examples include acrylic acid, methacrylic acid, maleic acid, maleic acid monomethyl ester, maleic anhydride, itaconic acid,
Examples include itaconic acid monomethyl ester, itaconic anhydride, fumaric acid, derivatives thereof, and metal salts of these acids. Also cyclic carboxylic acids, more specifically endo-bicyclo(2,2,1)-5-heptene-2,3-
Carboxylic acid anhydride, cis-4-cyclohexene-
1,2-carboxylic acid anhydrides, derivatives thereof, metal salts of these acids, and the like can be used. Alternatively, acrylic esters, epoxy group-containing compounds such as glycidyl methacrylate, etc. can also be used. The amount of unsaturated compound used in the present invention is:
For 100 parts by weight of polyolefin, preferably
0.01 to 5.0 parts by weight, particularly preferably 0.01 to 5.0 parts by weight
It is 2.0 parts by weight. The graft reaction between the polyolefin and the unsaturated compound is usually carried out by heating in the presence of an organic peroxide such as tert-butyl hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, benzoyl peroxide, etc. . The amount of organic peroxide added is 0.01 to 5.0 parts by weight per 100 parts by weight of polyolefin, especially
0.01 to 1.0 parts by weight is preferred. The unsaturated compound has a polymer weight [(a)+(b)+
(c)], it is preferably contained in a proportion of 0.01 to 2.0% by weight. Further, when producing a modified polyolefin, it is possible to simultaneously add magnesium oxide, aluminum hydroxide, magnesium hydroxide, antimony oxide, etc. to metalize the acid component, and it is also possible to add a filler. Generally, it is preferable to add a filler to unmodified polyolefin. Modified polyolefins are usually formed into pellets. Moreover, the unmodified polyolefin used in this invention
Examples of (b) include the aforementioned polyolefins. The same type of polyolefin used to obtain the modified polyolefin is preferably used. Conventionally known additives (antioxidants, ultraviolet absorbers, etc.) may be blended with the unmodified polyolefin. The powdered inorganic substance and modified polyolefin may each be used in the form of a masterbatch of unmodified polyolefin. As the elastomer (c) used in the present invention, a polymer having a lower tensile modulus (ASTMD-882-73) at room temperature than modified or unmodified polyolefin polymers is used. Specifically, various types of polyethylene, ethylene/propylene, ethylene/propylene/diene, ethylene/butene, styrene/butadiene, ethylene/acrylic acid, ethylene/ethyl acrylate, ionomer, ethylene/vinyl acetate copolymers, and liquid rubber. Also used are modified products and partially crosslinked products obtained by adding derivatives such as unsaturated acids, acid esters, metal salts, imides, amides, and unsaturated silane compounds to these compounds. Ethylene/propylene (diene) rubber or a modified version thereof is preferred over modified crystalline polypropylene. In addition, in these compositions, compatible polyamides such as nylon 6, nylon 12, polyester amide, polyether amide, polyester ether amide, etc. are added at a weight ratio of 1:1 to the total amount of modified polyolefin and elastomer. It can be used within the range. Calcium carbonate (heavy, light) used in the present invention
(d) is preferably a powder having an average particle diameter of 0.05 to 10 μm, particularly 0.5 to 5 μm, and a specific surface area of 0.1 to 100 m 2 /g, especially 1 to 30 m 2 /g. Preferably, calcium carbonate is not surface-treated. In addition to calcium carbonate, talc, mica,
Inorganic substances such as silicon oxide, silicon carbonates,
Hydroxides, oxides, etc. can also be added. In the adhesive polyolefin composition of the present invention, the proportions of each of the above-mentioned components are (a): 10 to 100% by weight of modified polyolefin, (b): 0 to 90% by weight of unmodified polyolefin, and (c) : Elastomer 0~
It can be obtained by mixing the calcium carbonate in an amount of 90% by weight (preferably 5 to 60% by weight) and (d): 5 to 50% by weight of the total composition. If the ratio of each component is outside the above range, the adhesiveness of the resulting composition will decrease. When the proportion of (a) is less than 10% by weight, the adhesiveness decreases, when the proportion of (b) is more than 90% by weight, the adhesiveness decreases, and when the proportion of (c) is more than 90% by weight, the adhesiveness decreases. decreases. When the proportion of (b) is less than 5% by weight, adhesiveness decreases and deformation due to thermal changes increases. Moreover, if it exceeds 50% by weight, there will be a drawback that it becomes brittle. The adhesive polyolefin composition of the present invention may contain various additives such as weathering (thermal) stabilizers,
A molding aid or the like may be added. The simplest mixing operation is to mix each of the above components at approximately 180 to 350°C, especially 220 to 350°C.
The mixture is melt-mixed in an extruder for about 1 to 10 minutes at a temperature of 270°C. Examples of the extruder include a single-screw or twin-screw extruder and a continuous mixer such as FCM. The effect of the present invention is further improved by performing a deaeration operation (venting) during melt-mixing.
This is because there is moisture attached to the surface of the powdered inorganic substance. By mixing each of the components (a) to (d) in the above-mentioned specific ratios, the composition of the present invention has a greater adhesive strength for thin metal sheets than conventionally known polyolefin resin-based adhesives. It has adhesive strength and exhibits extremely excellent properties as a sealing material, making it possible to obtain a thin battery with good long-term storage characteristics. If the blending ratio of each component in the composition is outside the above range, it will not be possible to obtain a composition that has adhesive properties, bending properties, and heat shock resistance. There are no particular limitations on the method for obtaining a thin battery using the above composition as a sealing material. A thin battery with excellent sealing performance can be obtained by sandwiching the laminate between the peripheral edges of a pair of laminated thin metal exterior plates and bonding them under heat. Further, the sheet or film described above can also be used as a three-layer sheet or a three-layer film in which the composition of the present invention is used as an adhesive layer and an intermediate layer made of an unmodified resin is provided in the middle. [Examples of the present invention] Next, Examples and Comparative Examples will be shown. In the following description, parts indicate parts by weight, and melt flow rate (MFR) was measured according to ASTM D1238. In addition, long-term storage stability was determined by a constant current discharge test at 200 μA after being left for 60 days after manufacture. The bending property test was conducted according to the IC card bending strength measurement method (DP7816/1). That is, the movable part was repeatedly moved left and right so that the amount of deflection as shown in FIG. 1 was 0 to 3 mm. The adhesive compositions of Examples and Comparative Examples are collectively shown in Table 1. (Materials used) Polyolefin 1 Polypropylene Ethylene-propylene block copolymer: Polypropylene (A) (J701H manufactured by Ube Industries, Ltd.) 2 Polyethylene Low density polyethylene: Polyethylene (B) (F222 manufactured by Ube Industries, Ltd.) 3 Ethylene - Propylene rubber Ethylene/propylene/ethylidene norbornene terpolymer: Ethylene propylene rubber (c)
(EP-57P manufactured by Japan Synthetic Rubber Co., Ltd.) Organic peroxide t-butyl hydroperoxide unsaturated compound 1 Alkenylsuccinic anhydride (15 carbon atoms) (DSA manufactured by Sanyo Chemical Co., Ltd.) [Example 1] (Method for making sealing material sheet) Polypropylene (A) [Tensile modulus: 14200Kg/
cm 2 ] 100 parts by weight, 2.0 parts by weight of alkenylsuccinic anhydride and 0.5 parts by weight of t-butyl hydroperoxide were dry blended, and the inner diameter was 30 mm.
Using a twin-screw extruder with L/D=17, the mixture was melt-kneaded at 250° C. and at a discharge rate of 2 kg/hour to form pellets. The pellets were dried by heating under reduced pressure to obtain modified polyolefin (1). After mixing 90 parts by weight of modified polyolefin (1) and 10 parts by weight of calcium carbonate [heavy, powdered with an average particle size of 2.1 μm and a specific surface area of 10.5 m 2 /g] in a blender,
The mixture was melt-kneaded for 2 minutes at 250° C. in a 50 mmφ vented single-screw extruder to obtain adhesive polyolefin composition pellets of approximately 2 mmφ×3 mm. An adhesive polyolefin sheet was prepared from this. From this sheet, with a punch blade, the outer diameter is 40 x 40 mm.
A circular sealant sheet with a width of 4 mm was prepared. (Creation method of positive electrode mixture) Manganese dioxide 332.9 mg, acetylene black
Methoxypolyethylene glycol monoacrylate (AM-
90G) 31.4mg, polyethylene glycol dimethacrylate (Shin Nakamura Chemical 9G) 10.7mg, dimethoxypolyethylene glycol (Asahi Denka LX-521)
Lithium perchlorate was dissolved in (concentration 0.75 m
mol/) solution and 0.067 mg of benzoyl peroxide were further mixed to prepare a positive electrode mixture. (Creation method of positive electrode) As a negative electrode current collector and exterior plate, the dimensions are 40 x 40 x
Spread the above positive electrode mixture 28x on 0.05mm stainless steel foil.
It was applied evenly to a size of 28 mm. This was pressure-molded and heated at 100° C. for 3 hours to create a positive electrode laminate A consisting of a positive electrode plate (300 μm thick) and an exterior plate. (Method for creating negative electrode and electrolyte diaphragm) As a negative electrode current collector and exterior plate, the dimensions are 40 x 40 x
Dimensions are 26 x 26 x 0.07 mm on 0.05 mm stainless steel foil.
lithium foil was crimped. As a composition for electrolyte, 18.4 mg of AM-90G,
A mixed solution of 6.0 mg of 9G, 25.6 mg of a solution of lithium perchlorate dissolved in LX-521 (concentration 0.75 mol/), and 0.1 mg of 2,2-dimethoxyacetophenone as a photosensitizer was prepared. . Apply 8μ of this electrolyte solution to the lithium metal disk,
Using a 250 W ultra-high pressure mercury lamp, irradiation was performed for 3 minutes at an illumination intensity of 5 mW/cm to form a cured film with a thickness of 50 μm, thereby creating a laminate B of a current collector/exterior plate, a negative electrode, and an electrolyte diaphragm. (Assembling the battery) The above laminates A and B are stacked, the annular sealing sheet is sandwiched between the outer periphery of the outer plate, and heat and pressure bonded (180°C, 3Kg/cm 2 , 3 minutes) to form a thin battery. assembled. The results of the battery discharge test are shown in FIG. 2 below. In addition, regarding the battery, bending test
Even after 5,000 cycles, no abnormality was observed in the sealing part or electrical properties. [Example 2] Modified polyolefin (1) and polypropylene (A)
A thin battery was assembled in the same manner as in Example 1 by using these melt-kneaded products in a combination system with calcium carbonate and calcium carbonate. Note that the bending test results were the same as in Example 1. [Example 3] In Example 2, part of the polypropylene (A) was replaced with ethylene propylene rubber (C) [EPR
(C)] A thin battery was assembled in the same manner as in Example 2, except that the battery was used. Note that the bending test results were the same as in Example 1. [Example 4] Except for using unmodified polyethylene (B) [PE (B)] in place of EPR (C) in Example 3,
A thin battery was assembled in the same manner as in Example 3. Note that the bending test results were the same as in Example 1. [Comparative Example 1] A thin battery was assembled in the same manner as in Example 1, except that a kneaded product of polypropylene (A) and calcium carbonate was used. In addition, when we conducted a bending test,
Peeling was observed at the sealing part after 1000 cycles. [Comparative Example 2] Example 1 except that a kneaded product of modified polypropylene (1) and ethylene propylene rubber (C) was used.
A thin battery was assembled in the same manner. Note that the bending test results were the same as in Comparative Example 1. 【table】

【図面の簡単な説明】[Brief explanation of the drawing]

第1図は本発明におけるベンデイング特性試験
の方法を示したものである。第2図は本発明によ
る薄形電池の電池放電試験の結果を示す特性図で
あり、は実施例1による薄形電池の、は実施
例2による薄形電池の、は実施例3による薄形
電池の、は実施例4による薄形電池の、は比
較例1による薄形電池の、は比較例2による薄
形電池の、それぞれの200μAの定電流放電試験結
果である。
FIG. 1 shows a method for testing bending characteristics in the present invention. FIG. 2 is a characteristic diagram showing the results of a battery discharge test of the thin battery according to the present invention, where is the thin battery according to Example 1, is the thin battery according to Example 2, and is the thin battery according to Example 3. 200 μA constant current discharge test results for the thin battery according to Example 4, the thin battery according to Comparative Example 1, and the thin battery according to Comparative Example 2.

Claims (1)

【特許請求の範囲】 1 集電体を兼ねた対向した一対の金属薄板から
なる外装板の内部に、正極と負極との中間に電解
質を含むセパレータあるいは固体電解質の隔膜を
形成し、外装板の周縁を封口材で密封した薄形電
池であつて、前記封口材として、下記(a)乃至(d)の
各成分のうち少なくとも2成分を含有しており、
各成分の配合割合は、ポリマー重量中(a)が10〜
100重量%、(b)が0〜90重量%、(c)が0〜90重量
%であり、全組成物重量中(d)が5〜50重量%であ
る接着性ポリオレフイン組成物を用いることを特
徴とする薄形電池。 (a) ポリオレフインとアルケニルコハク酸類また
は式CR1R2=CR3−CO−R4(式中、R1,R2及
びR3はHまたは炭素数1〜10のアルキル基で
あり、R4はベンゾトリアゾール、フタルイミ
ド、オルソスルホベンゾイミド、1,8−ナフ
タルイミド、コハク酸イミド、ラクタム類及び
これらの誘導体からHを除いた残基である。)
で表わされる不飽和化合物とをグラフト反応し
て得られる変性ポリオレフイン。 (b) 未変性のポリオレフイン (c) エラストマー (d) 炭酸カルシウム
[Claims] 1. A separator containing an electrolyte or a solid electrolyte diaphragm is formed between a positive electrode and a negative electrode inside an exterior plate consisting of a pair of opposing thin metal plates that also serves as a current collector, and A thin battery whose periphery is sealed with a sealing material, the sealing material containing at least two of the following components (a) to (d),
The blending ratio of each component is from 10 to 10% of (a) in the weight of the polymer.
Use an adhesive polyolefin composition in which (b) is 0 to 90% by weight, (c) is 0 to 90% by weight, and (d) is 5 to 50% by weight based on the total composition weight. A thin battery featuring (a) Polyolefin and alkenylsuccinic acids or the formula CR 1 R 2 = CR 3 -CO-R 4 (wherein, R 1 , R 2 and R 3 are H or an alkyl group having 1 to 10 carbon atoms, and R 4 is a residue obtained by removing H from benzotriazole, phthalimide, orthosulfobenzimide, 1,8-naphthalimide, succinimide, lactams, and their derivatives.)
A modified polyolefin obtained by a graft reaction with an unsaturated compound represented by (b) Unmodified polyolefin (c) Elastomer (d) Calcium carbonate
JP62076025A 1987-03-31 1987-03-31 Thin type battery Granted JPS63244551A (en)