JPH0454754B2 - - Google Patents

Info

Publication number
JPH0454754B2
JPH0454754B2 JP20626482A JP20626482A JPH0454754B2 JP H0454754 B2 JPH0454754 B2 JP H0454754B2 JP 20626482 A JP20626482 A JP 20626482A JP 20626482 A JP20626482 A JP 20626482A JP H0454754 B2 JPH0454754 B2 JP H0454754B2
Authority
JP
Japan
Prior art keywords
sulfur trioxide
carbon
steel
chamber
containing fluid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
JP20626482A
Other languages
Japanese (ja)
Other versions
JPS5996283A (en
Inventor
Josefu Setsuchinerii Uiriamu
Edowaado Kurasen Harorudo
Kaaru Torei Miruton
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dow Chemical Co
Original Assignee
Dow Chemical Co
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dow Chemical Co filed Critical Dow Chemical Co
Priority to JP20626482A priority Critical patent/JPS5996283A/en
Publication of JPS5996283A publication Critical patent/JPS5996283A/en
Publication of JPH0454754B2 publication Critical patent/JPH0454754B2/ja
Granted legal-status Critical Current

Description

【発明の詳細な説明】[Detailed description of the invention]

先行技術の処理法により、固体材料例えば金属
またはガラスの表面には種々の形態の残留炭素の
層を有していることがある。このような表面炭素
は次の表面処理を妨害し得る。例えば、鋼板もし
くはシートはその表面に金属を圧延する際に使用
した滑剤に由来する残留有機化合物を有してい
る。この炭素は鋼を焼なましした後は除去するの
が特に難しい。鋼を後程処理例えば燐酸塩処理も
しくは塗装する場合、鋼の表面上の残留炭素は有
効な処理を妨害し、それにより次の適用において
鋼の腐食の可能性を増大するものである。これま
でに金属表面を清浄にし、かつ残留炭素を除去す
る努力において酸もしくはアルカリ洗滌が使用さ
れていた。しかしながら、酸洗滌は、危険である
点に加えて、特色として時間がかかり、またアル
カリ洗滌は通常上昇した温度で行われ、そのため
に一層エネルギー強化となる。 本発明はその上に残留炭素の層を有する金属、
ガラスもしくはその他の表面を処理する方法を提
供するものである。本発明は炭素層を有する固体
表面から該層を除去する方法に係り、その特徴と
するところは該表面を三酸化硫黄含有流体と接触
させ、そして次に該表面を洗いすすぐことにあ
る。 本発明の方法は好ましくは本質的に無水の条件
下で実施される。この処理により、炭素層は有効
に除去される。 本発明はまた表面を三酸化硫黄含有流体と接触
させ、次に該表面を洗いすすぐことにより処理し
た残留炭素を実質的に含有しない固体表面を有す
る製造物品にも係るものである。 本発明はまた実質的に残留炭素を含有していな
い、かつ表面を三酸化硫黄含有流体と接触させ、
該表面を洗いすすぎし、そして該表面を不動化
(passivating)溶液で処理することによつて処理
された固体表面を有する製造物品に係る。 炭素は種々の有機化合物あるいは不活性の原子
価零の炭素(無定形もしくはグラフアイト形)の
形態で存在する。有機化合物は先行処理から表面
上に残留するグリースもしくはオイルから由来す
るものである。不活性炭素は固体表面の熱処理の
結果として有機化合物の分解から生じる。金属表
面で、炭素層は例えば50オングストローム単位の
深さに不規則な表面に結合されている。 使用される三酸化硫黄含有流体は気体状三酸化
硫黄単独または液体系(ガスまたは非水液体)の
活性成分としてであつてもよい。流体は洗浄化す
べき表面に三酸化硫黄を本発明の方法で作用する
ような形態で運搬するものでなければならない。
好ましくは流体は三酸化硫黄と実質的に非反応性
である。液体系の例にはガス例えば乾燥空気また
は窒素および非水性液体例えば発煙硫酸および有
機液体例えば塩素化溶媒およびふつ素化溶媒が包
含される。 好ましくは、固体表面と三酸化硫黄含有流体と
の接触は本質的に水のない条件下で達成されなけ
ればならない。固体表面が湿つているときは、表
面は最初に例えば上昇した温度に加熱して残留表
面水分を除去することにより乾燥することができ
る。好ましくは、固体表面と三酸化硫黄含有流体
との接触面のまわりの雰囲気が本質的に無水でな
ければならない。例えば、接触を容器中で行うべ
きときは、容器内の雰囲気を三酸化硫黄含有流体
と固体表面との接触前に水蒸気を減少させるよう
パージすることができる。 本発明の方法で利用される接触時間は除去すべ
き炭素層の所望の量および液体中の三酸化硫黄の
濃度に左右される。一般には、三酸化硫黄の濃度
が高いほど、所定量の表面炭素を除去するのに要
する時間は短くなる。実験では、炭素の大部分は
僅か二、三秒の接触で本方法により除去されるこ
とがわかつた。 表面を三酸化硫黄と接触した後、表面を液体
(ガスまたは液)でフラツシ、清掃あるいは他の
方法で洗いすすぎする。洗いすすぎ液体は水をベ
ースとする液が好ましい。洗いすすぎ工程はまた
表面の後処理プロセス第一工程でもあり得る。 清掃すべき固体が鋼または鋼合金であるとき
は、三酸化硫黄含有流体と接触した後の金属表面
は、例えば鋼表面に赤銹が急速に形成されること
により示されるように高度に活性化されているこ
とが認められた。従つて、本発明の方法では好ま
しくは三酸化硫黄含有流体で処理された鋼表面を
次に不動化溶液と接触させる。不動化溶液は金属
表面の酸化を防止あるいは他に抑制し、かくして
表面を安定化するものである。不動化溶液は例え
ば任意の既知の金属表面錯生成体例えばキレート
剤例えば処理された金属表面を有効に不動化する
エチレンジアミン四酢酸あるいはヒドロキシエチ
ルイミドジアセテート、ナイトライト、ナイトレ
ートおよびクロメートから調製され得る。不動化
溶液はまた洗いすすぎ工程での液体としても役立
つものである。好ましくは、不動化溶液と接触さ
せた直後に水洗を使用する。 ほとんどの適用例にとつて好ましいものである
が、本発明の有用性を得るのに鋼表面を不動化す
るのは必要ではない。例えば、鋼を燐酸塩処理に
おいて燐酸塩処理を実施する清浄な、化学的に均
一な活性表面を有するのが望ましい。 本発明の方法ではかかる鋼表面が提供される。 本発明の方法は除去が所望される残留炭素層を
有する固体表面(金属および窯業製品例えばガラ
スを包含する)の種々なものに適用可能である。
本発明の方法では、残留表面炭素の有効な除去の
ための迅速な、安価な、簡便な操作法が提供され
る。方法はバツチ操作であるいは好ましくは固体
表面を三酸化硫黄含有体の帯域を通過させる連続
ライン操作で実施することができる。 実施例 以下に記載の実施例では、他に特定しない限り
次の装置を用いて実施した。固体表面と接触させ
るのに三酸化硫黄ガスを提供するために、水蒸気
加熱浴中の三酸化硫黄蒸発器を使用した。該蒸発
器を4ステンレス鋼/ガラス処理室に連結し、
該室に処理すべき固体の試料を入れた。三酸化硫
黄蒸発器を加熱し、そして連結管を4の室に開
くことにより、SO3蒸気を処理室中に送入した。
不動化溶液または水洗いすすぎ液は直接処理室中
に供給した。 全ての実施例において、表面炭素をオージエ
(Auger)電子分光分析法、当業者間で周知の分
光分析法により測定した。要点は刊行物「メソ
ヅ・アンド・フエノミナ、メソヅ・オブ・サーフ
エイス・アナリシス」(Methods and
Phenomena,Methods of Surface Analysis)、
第1巻、第15章、エルスフイエル・サイエンテイ
フイツク・パブリシング・カンパニー(Elsevir
Scientific Publishing Company)、1975年に掲
載されている。加えて、本発明に従つて処理され
た全ての金属試料では、該処理金属試料の表面が
水で容易に湿潤させることが認められた。該表面
のの1滴の水は速やかにフイルムを形成し、これ
が実質的に清浄な金属表面の特色である。 実施例 1−5 アルミニウム箔試料を処理室に入れ、そして窒
素フラツシ後に約5.4gのSO3を室内に蒸発させ
た。特定の接触時間後に水を急速に室内に流し入
れてSO3を溶解し、そしてクーポンを洗いすすぎ
した。多重オージエ分光分析測定の結果を第表
に示す。
Due to prior art processing methods, the surface of solid materials such as metal or glass may have layers of residual carbon in various forms. Such surface carbon can interfere with subsequent surface treatments. For example, a steel plate or sheet has residual organic compounds on its surface derived from the lubricant used when rolling the metal. This carbon is particularly difficult to remove after annealing the steel. If the steel is subsequently treated, such as phosphating or painting, residual carbon on the surface of the steel will interfere with effective treatment, thereby increasing the likelihood of corrosion of the steel in subsequent applications. In the past, acid or alkaline cleaning has been used in efforts to clean metal surfaces and remove residual carbon. However, pickling, in addition to being dangerous, is characteristically time consuming and alkaline cleaning is usually carried out at elevated temperatures, which makes it more energy intensive. The present invention comprises a metal having a layer of residual carbon thereon;
A method of treating glass or other surfaces is provided. The present invention relates to a method for removing a carbon layer from a solid surface, characterized by contacting the surface with a sulfur trioxide-containing fluid and then rinsing the surface. The process of the invention is preferably carried out under essentially anhydrous conditions. This treatment effectively removes the carbon layer. The present invention also relates to an article of manufacture having a solid surface substantially free of residual carbon that is treated by contacting the surface with a sulfur trioxide-containing fluid and then washing and rinsing the surface. The present invention also includes contacting the surface with a sulfur trioxide-containing fluid that is substantially free of residual carbon;
An article of manufacture having a solid surface treated by washing and rinsing the surface and treating the surface with a passivating solution. Carbon exists in the form of various organic compounds or inert zero-valent carbon (amorphous or graphite form). Organic compounds originate from grease or oil remaining on the surface from previous processing. Inert carbon results from the decomposition of organic compounds as a result of heat treatment of solid surfaces. On the metal surface, the carbon layer is bonded to an irregular surface to a depth of, for example, 50 angstroms. The sulfur trioxide-containing fluid used may be gaseous sulfur trioxide alone or as the active ingredient in a liquid system (gas or non-aqueous liquid). The fluid must be capable of delivering sulfur trioxide to the surface to be cleaned in such a form as to be effective in the method of the present invention.
Preferably the fluid is substantially non-reactive with sulfur trioxide. Examples of liquid systems include gases such as dry air or nitrogen and non-aqueous liquids such as fuming sulfuric acid and organic liquids such as chlorinated and fluorinated solvents. Preferably, contacting the solid surface with the sulfur trioxide-containing fluid must be accomplished under essentially water-free conditions. If the solid surface is wet, the surface can be first dried, for example by heating to an elevated temperature to remove residual surface moisture. Preferably, the atmosphere around the interface between the solid surface and the sulfur trioxide-containing fluid should be essentially anhydrous. For example, when contacting is to occur in a container, the atmosphere within the container can be purged to reduce water vapor prior to contacting the sulfur trioxide-containing fluid with the solid surface. The contact time utilized in the method of the invention depends on the desired amount of carbon layer to be removed and the concentration of sulfur trioxide in the liquid. Generally, the higher the concentration of sulfur trioxide, the shorter the time required to remove a given amount of surface carbon. Experiments have shown that most of the carbon is removed by this method after only a few seconds of contact. After contacting the surface with the sulfur trioxide, the surface is flushed, cleaned or otherwise rinsed with a liquid (gas or liquid). Preferably, the washing and rinsing liquid is water-based. The washing and rinsing step may also be the first step in the surface post-treatment process. When the solid to be cleaned is steel or steel alloys, the metal surface after contact with the sulfur trioxide-containing fluid becomes highly activated, as indicated by the rapid formation of red rust on the steel surface, for example. It was recognized that Therefore, in the method of the present invention, preferably the steel surface treated with the sulfur trioxide-containing fluid is then contacted with an immobilization solution. The passivating solution prevents or otherwise inhibits oxidation of the metal surface, thus stabilizing the surface. The immobilization solution may be prepared, for example, from any known metal surface complexing agent such as a chelating agent such as ethylenediaminetetraacetic acid or hydroxyethylimide diacetate, nitrite, nitrate and chromate, which effectively immobilizes the treated metal surface. . The immobilization solution also serves as a liquid in the washing and rinsing process. Preferably, a water wash is used immediately after contacting with the immobilization solution. Although preferred for most applications, it is not necessary to immobilize the steel surface to obtain the utility of the present invention. For example, in phosphating steel, it is desirable to have a clean, chemically uniform active surface on which to perform the phosphating process. The method of the invention provides such a steel surface. The method of the present invention is applicable to a variety of solid surfaces (including metals and ceramic products such as glass) having residual carbon layers that are desired to be removed.
The method of the present invention provides a fast, inexpensive, and simple procedure for effective removal of residual surface carbon. The process can be carried out in a batch operation or preferably in a continuous line operation in which the solid surface is passed through a zone of sulfur trioxide containing material. EXAMPLES The examples described below were carried out using the following equipment unless otherwise specified. A sulfur trioxide evaporator in a steam heating bath was used to provide sulfur trioxide gas in contact with the solid surface. connecting the evaporator to four stainless steel/glass processing chambers;
A sample of the solid to be treated was placed in the chamber. SO 3 vapor was introduced into the processing chamber by heating the sulfur trioxide evaporator and opening the manifold into chamber 4.
The immobilization solution or water rinse solution was fed directly into the processing chamber. In all examples, surface carbon was measured by Auger electron spectroscopy, a spectroscopic method well known to those skilled in the art. The main points are summarized in the publication ``Methods and Phenomena, Methods of Surf-Eighth Analysis.''
Phenomena, Methods of Surface Analysis)
Volume 1, Chapter 15, Elsevir Scientific Publishing Company
Scientific Publishing Company), 1975. Additionally, for all metal samples treated according to the present invention, it was observed that the surface of the treated metal samples was easily wettable with water. A drop of water on the surface quickly forms a film, which is characteristic of a substantially clean metal surface. Examples 1-5 Aluminum foil samples were placed in a processing chamber and approximately 5.4 g of SO 3 was evaporated into the chamber after nitrogen flushing. After the specified contact time, water was rapidly flushed into the chamber to dissolve the SO 3 and wash and rinse the coupons. The results of the multiple Auger spectroscopy measurements are shown in Table 1.

【表】 これらの実施例により、本発明の方法による表
面炭素の有効な除去が実証される。 実施例 6 冷圧延鋼パネルを処理室中で60℃に平衡させ
た。室を窒素フラツシおよび排気した後、液状
SO3の2mlを室に蒸発させた。SO3蒸気を窒素で
ブラツシする前に20分間SO3を温いクーポンと接
触させておき、そして脱イオン化した水でクーポ
ンを洗いすすぎした。これらのクーポンを乾燥
し、オージエ分光分析法にかけた。未処理の対照
パネルも処理試料と比較のために検査した。得ら
れたオージエ深度プロフイルを検討すると、表面
炭素が約25重量%から2重量%未満に低減してい
ることがわかつた。 実施例 7−9 軟鋼クーポン(2.5cm×7cm×厚さ3mm)をト
ルエン洗滌し、アセトンで洗いすすぎし、そして
10分間10%HClで酸洗いした。これらを乾燥し、
処理室に懸垂した。室を窒素フラツシし、そして
10.8gのSO3を4容量に蒸発させた。SO3蒸気
との接触時間はSO3を窒素気流で吹出す前10分間
であつた。3枚のクーポンを各スルホン化で処理
し、そして3枚のクーポンの各バツチを直接別異
の洗いすすぎ液に入れた。 3種の洗いすすぎ液は実施例7脱イオン化した
水、実施例80.01N NaOHおよび実施例9ヒドロ
キシエチルイミドジアセテート(HEIDA)の5
%溶液であつた。クーポンを10分間洗いすすぎ溶
液中でかくはんした。 脱イオン化した洗いすすぎの場合、クーポン表
面はなお洗いすすぎ液中にある間に変色し始め
た。これが黒色に変り、洗いすすぎ液から出すと
赤銹を形成し始めた。 0.01N NaOHおよび5%HEIDA溶液中では当
初のクーポン変色は認められなかつた。全クーポ
ンをそれぞれの洗いすすぎ液から取り出し、5分
間の新たな脱イオン化した水の洗いすすぎをし、
そしてつるして風乾した。0.01N NaOHで洗い
すすいだクーポンはごく僅か銹を生じたが、一方
HEIDA浴からの3枚のクーポンは清浄で、銹が
なくかつ光つたまゝであつた。 洗いすすぎ工程後の軟鋼クーポンについてオー
ジエ分光分析測定を行つた。結果を第表に示
す。
TABLE These examples demonstrate the effective removal of surface carbon by the method of the present invention. Example 6 Cold rolled steel panels were equilibrated to 60°C in a processing chamber. After flushing and evacuating the chamber with nitrogen, the liquid
2 ml of SO 3 was evaporated into the chamber. The SO 3 was allowed to contact the warm coupons for 20 minutes before brushing the SO 3 vapor with nitrogen and washing and rinsing the coupons with deionized water. These coupons were dried and subjected to Augier spectroscopy. An untreated control panel was also examined for comparison with the treated samples. Examination of the resulting Augier depth profiles revealed a reduction in surface carbon from about 25% by weight to less than 2% by weight. Example 7-9 Mild steel coupons (2.5 cm x 7 cm x 3 mm thick) were washed with toluene, rinsed with acetone, and
Pickled with 10% HCl for 10 minutes. Dry these
It was suspended in the processing chamber. flush the chamber with nitrogen, and
10.8g SO 3 was evaporated to 4 volumes. The contact time with the SO 3 vapor was 10 minutes before the SO 3 was blown out with a nitrogen stream. Three coupons were treated with each sulfonation, and each batch of three coupons was placed directly into a separate wash rinse solution. The three wash rinse solutions were Example 7 deionized water, Example 8 0.01N NaOH, and Example 9 Hydroxyethylimide diacetate (HEIDA).
% solution. The coupons were washed and agitated in the rinse solution for 10 minutes. In the case of the deionized wash rinse, the coupon surface began to discolor while still in the wash rinse. This turned black and began to form a red stain when removed from the rinse solution. No initial coupon discoloration was observed in 0.01N NaOH and 5% HEIDA solution. Remove all coupons from their respective rinse solutions and rinse with fresh deionized water for 5 minutes;
Then I hung it up to air dry. Coupons washed and rinsed with 0.01N NaOH produced very little rust;
The three coupons from the HEIDA bath were clean, free of rust, and shiny. Auger spectroscopy measurements were performed on the mild steel coupons after the washing and rinsing process. The results are shown in Table 1.

【表】【table】

【表】 実施例 10−14 鋼シート金属試料(3″×4″)(7.6cm×10.2cm)
のSO3処理を処理室で行つた。処理すべき試料を
室の開放部に懸垂し、室を水銀圧2−3mlに排気
し、約4gのSO3を真空内に蒸発させ、そして5
分間クーポンと接触させ、そして最後に依然とし
て鋼および残留SO3蒸気が入つている容器中に直
接洗いすすぎを適用した。洗いすすぎは種々の量
のキラント(chelant)を得た。各例の洗いすす
ぎに十分なNaOHを加えて洗いすすぎ液が残留
SO3と混合したときに形成される硫酸を中和し
た。この洗いすすぎ液と1分間接触した後、クー
ポンをとり出し、脱イオン化した水で洗いすすぎ
しそして風乾した。 清浄化した表面のオージエ分光分析の結果を他
の実験観察と共に第表に提示する。
[Table] Example 10-14 Steel sheet metal sample (3″ x 4″) (7.6cm x 10.2cm)
SO 3 treatment was carried out in a treatment chamber. The sample to be processed is suspended in the opening of the chamber, the chamber is evacuated to 2-3 ml of mercury pressure, approximately 4 g of SO 3 is evaporated into the vacuum, and
in contact with the coupon for minutes and finally applied a wash rinse directly into the container still containing the steel and residual SO 3 vapor. The wash rinses yielded varying amounts of chelant. Add enough NaOH to each wash and rinse so that the wash and rinse solution remains
Neutralized the sulfuric acid formed when mixed with SO 3 . After 1 minute of contact with this rinse solution, the coupons were removed, rinsed with deionized water, and air dried. The results of Augier spectroscopy of the cleaned surfaces are presented in Table 1 along with other experimental observations.

【表】 実施例 15 車体鋼のシート鋼列の小さい切片(3″×1″×
1/32″)(7.6cm×2.54cm×0.08cm)を截断し、そ
して2のガラス容器に入れた。この室を窒素で
フラツシし、そして60℃で排気した。液状SO3
(2ml)を室に注入した。鋼試料およびSO3を、
処理室からSO3蒸気をフラツシする前に、20分間
接触下に保持し、そして脱イオン化した水で洗い
すすぎした。鋼試料を更に新たな脱イオン化した
水で洗いすすぎし、そして窒素乾燥した。オージ
エ分析を第表に提示する。 第表 鋼シート−SO3蒸気清浄−炭素の表面濃度実施例No. 炭素(重量%) 比較D 44 15 2 実施例 16−20 自動車鋼を代表する軟鋼シートから1インチ平
方(6.45cm2)クーポンを截断した。ガラスビン処
理室を使用し、この室は大量の窒素で直ちにフラ
ツシした。圧力により(真空乃至大気圧)保持さ
れたゴム栓もまた直ちに除去することができた。
この窒素フラツシングおよび迅速な栓除去によ
り、SO2−鋼接触時間は10秒ほど短く低減するこ
とができた。全ての処理は試料および処理室を60
℃に平衡した後に実施した。液体SO3を直接処理
室に注入し、室の温い底部から蒸発させた。熱は
室表面下および直接触れている加熱プレートによ
り供給された。試料を室からとり出し、そして脱
イオン化した水で洗いすすぎした。 第表から、10秒乃至20分の期間処理した試料
で同様なレベルの炭素除去が得られることがわか
つた。これらのデータから、比較的短時間のSO3
曝しが表面炭素を除去するのに有効であることが
わかる。
[Table] Example 15 Small section of sheet steel row of car body steel (3″×1″×
1/32") (7.6 cm x 2.54 cm x 0.08 cm) and placed in a 2 glass container. The chamber was flushed with nitrogen and evacuated at 60°C. Liquid SO 3
(2 ml) was injected into the chamber. steel sample and SO 3 ,
It was held in contact for 20 minutes and rinsed with deionized water before flushing the SO 3 vapor from the processing chamber. The steel samples were further rinsed with fresh deionized water and dried with nitrogen. The Augier analysis is presented in Table 1. Table Steel Sheet - SO 3 Steam Cleaning - Carbon Surface Concentration Example No. Carbon (wt%) Comparison D 44 15 2 Example 16-20 1 inch square (6.45 cm 2 ) coupon from a mild steel sheet representative of automotive steel was cut off. A glass vial processing chamber was used and the chamber was immediately flushed with copious amounts of nitrogen. Rubber stoppers held under pressure (vacuum to atmospheric pressure) could also be immediately removed.
With this nitrogen flushing and rapid plug removal, the SO2 -steel contact time could be reduced to as little as 10 seconds. All processing requires 60 samples and processing chambers.
It was carried out after equilibration to °C. Liquid SO 3 was injected directly into the treatment chamber and allowed to evaporate from the warm bottom of the chamber. Heat was provided by heating plates below and in direct contact with the chamber surface. The sample was removed from the chamber and rinsed with deionized water. From the table it can be seen that similar levels of carbon removal were obtained for samples treated for periods of 10 seconds to 20 minutes. From these data, it is clear that SO 3 for a relatively short period of time
It can be seen that exposure is effective in removing surface carbon.

【表】 実施例 21 黒色プレート鋼試料(8″×33/8″×0.006″) (20.3cm×8.59cm×0.15mm)を、3.5室に該試料
を入れ、室を窒素フラツシで乾燥し、室を排気し
そして液体SO3を45℃に保持した室に注入するこ
とにより処理した。接触時間は5分間であり、次
いで脱イオン化した水で洗いすすぎした。表面炭
素重量%はオージエ分光分析法で測定して85%か
ら5%に低減した。 実施例 22−23 黒色プレート鋼試料(1″×33/8″×0.006″) (2.54cm×8.59cm×0.15mm)を3.5室(水蒸気加
熱)中同時に2個処理し、この室は各処理のため
に乾燥し、排気した。真空下の試料を、液体SO3
の4ml(7.2g)を直接室に注入する前に、50℃
で室内で平衡化させた。10秒および1分の接触時
間で窒素フラツシを使用してSO3蒸気を除去、希
釈した。試料を脱イオン化した水で洗いすすぎ
し、そしてオージエ分析前に乾燥した。分析値を
第表に示す実施例22−23については6個の試料
の平均値および比較については2個の試料の平均
値)。 第表 SO3処理した黒色プレート鋼についての炭素重量
%実施例No. 炭素(重量%) 比較E 65.0 22(10秒処理) 10.0 23(1分処理) 8.5 実施例 24 ガラス試料約1/4平方インチ(0.41cm2)を、試
料の入つたガラスフラスコ中にSO3液体2mlを注
入することにより、三酸化硫黄と接触させた。蒸
発されたSO3と10分の接触後、フラスコを窒素で
フラツシし、ガラス試料を水で洗いすすぎし、そ
して風乾した。表面炭素をオージエ分光分析法に
より分析した。 処理ガラス試料の表面上のC重量%は10%であ
つた。未処理ガラス試料の表面上のC重量%は40
%であつた。 実施例 25−27 これらの実施例では、三酸化硫黄を塩素化溶媒
に溶解した。冷圧延鋼シートの試料を第表に記
載した処理に受けしめ、次いで表面炭素を測定し
た。データから本発明の方法により達成される改
善された炭素除去が実証される。
[Table] Example 21 A black plate steel sample (8″ x 33/8″ x 0.006″) (20.3 cm x 8.59 cm x 0.15 mm) was placed in chamber 3.5, and the chamber was dried with a nitrogen flush. The chamber was evacuated and treated by injecting liquid SO 3 into the chamber maintained at 45° C. Contact time was 5 minutes, followed by a rinse with deionized water. Surface carbon weight percent was determined by Augier spectroscopy. Example 22-23 A black plate steel sample (1″ x 33/8″ x 0.006″) (2.54 cm x 8.59 cm x 0.15 mm) was heated in 3.5 chambers (steam heating ) and the chamber was dried and evacuated for each treatment. Sample under vacuum, liquid SO 3
50℃ before injecting 4 ml (7.2 g) directly into the chamber.
and equilibrated indoors. SO 3 vapor was removed and diluted using a nitrogen flush with contact times of 10 seconds and 1 minute. Samples were rinsed with deionized water and dried before Auger analysis. The analytical values are shown in Table 1 (for Examples 22-23, the average value of 6 samples and for comparison, the average value of 2 samples). Table Carbon weight % for SO 3 treated black plate steel Example No. Carbon (weight %) comparison E 65.0 22 (10 seconds treatment) 10.0 23 (1 minute treatment) 8.5 Example 24 Glass sample approx. 1/4 square An inch (0.41 cm 2 ) was contacted with sulfur trioxide by injecting 2 ml of SO 3 liquid into the glass flask containing the sample. After 10 minutes of contact with the evaporated SO3 , the flask was flushed with nitrogen, the glass sample rinsed with water, and air dried. Surface carbon was analyzed by Augier spectroscopy. The weight percent C on the surface of the treated glass sample was 10%. The weight percent C on the surface of the untreated glass sample is 40
It was %. Examples 25-27 In these examples, sulfur trioxide was dissolved in a chlorinated solvent. Samples of cold rolled steel sheets were subjected to the treatments listed in the table and the surface carbon was then measured. The data demonstrate the improved carbon removal achieved by the method of the present invention.

【表】 試料を脱イオン化し
た水で洗いすすい
だ。
[Table] Deionize the sample
Rinse with water
is.

【表】 た水で洗いすすい
だ。
[Front] Wash and rinse with tap water
is.

Claims (1)

【特許請求の範囲】 1 炭素層を有する固体表面から炭素層を除去す
る方法において、該表面を三酸化硫黄含有流体と
接触させ、そして次に該表面を洗いすすぎするこ
とを特徴とする上記方法。 2 三酸化硫黄含有流体が三酸化硫黄からなる特
許請求の範囲第1項記載の方法。 3 三酸化硫黄含有流体が乾燥空気または窒素で
ある特許請求の範囲第1記載の方法。 4 三酸化硫黄含有流体が塩素化炭化水素溶媒で
ある特許請求の範囲第1項記載の方法。 5 接触工程を本質的に無水の条件下で実施する
特許請求の範囲第1項記載の方法。 6 洗いすすぎ工程を表面を水で洗浄することに
よつて達成する特許請求の範囲第1項記載の方
法。 7 洗いすすぎ工程を表面を不動化溶液と接触さ
せることによつて達成する特許請求の範囲第1項
記載の方法。 8 表面が金属である特許請求の範囲第1項記載
の方法。 9 表面がセラミツクである特許請求の範囲第1
項記載の方法。 10 炭素層を有する固体表面から炭素層を除去
する方法において、該表面を三酸化硫黄含有流体
と接触させ、そして次に該表面を不動化溶液と接
触させることを特徴とする上記方法。 11 不動化溶液がキレート化剤を含有する特許
請求の範囲第10項記載の方法。 12 表面が金属である特許請求の範囲第10項
記載の方法。 13 表面がセラミツクである特許請求の範囲第
10項記載の方法。
Claims: 1. A method for removing a carbon layer from a solid surface having a carbon layer, characterized in that the surface is contacted with a sulfur trioxide-containing fluid and then the surface is washed and rinsed. . 2. The method according to claim 1, wherein the sulfur trioxide-containing fluid comprises sulfur trioxide. 3. The method according to claim 1, wherein the sulfur trioxide-containing fluid is dry air or nitrogen. 4. The method of claim 1, wherein the sulfur trioxide-containing fluid is a chlorinated hydrocarbon solvent. 5. The method of claim 1, wherein the contacting step is carried out under essentially anhydrous conditions. 6. The method according to claim 1, wherein the washing and rinsing step is achieved by washing the surface with water. 7. The method of claim 1, wherein the washing and rinsing step is accomplished by contacting the surface with an immobilizing solution. 8. The method according to claim 1, wherein the surface is metal. 9 Claim 1 in which the surface is made of ceramic
The method described in section. 10. A method for removing a carbon layer from a solid surface having a carbon layer, characterized in that the surface is contacted with a sulfur trioxide-containing fluid and then the surface is contacted with an immobilization solution. 11. The method of claim 10, wherein the immobilization solution contains a chelating agent. 12. The method according to claim 10, wherein the surface is metal. 13. The method according to claim 10, wherein the surface is ceramic.
JP20626482A 1982-11-26 1982-11-26 Removal of carbon from solid surface Granted JPS5996283A (en)