JPH0459687B2 - - Google Patents

Info

Publication number
JPH0459687B2
JPH0459687B2 JP58083359A JP8335983A JPH0459687B2 JP H0459687 B2 JPH0459687 B2 JP H0459687B2 JP 58083359 A JP58083359 A JP 58083359A JP 8335983 A JP8335983 A JP 8335983A JP H0459687 B2 JPH0459687 B2 JP H0459687B2
Authority
JP
Japan
Prior art keywords
thin film
metal thin
film
magnetic recording
ferromagnetic metal
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
JP58083359A
Other languages
Japanese (ja)
Other versions
JPS59207424A (en
Inventor
Koichi Shinohara
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Panasonic Holdings Corp
Original Assignee
Matsushita Electric Industrial Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Matsushita Electric Industrial Co Ltd filed Critical Matsushita Electric Industrial Co Ltd
Priority to JP58083359A priority Critical patent/JPS59207424A/en
Publication of JPS59207424A publication Critical patent/JPS59207424A/en
Publication of JPH0459687B2 publication Critical patent/JPH0459687B2/ja
Granted legal-status Critical Current

Description

【発明の詳細な説明】[Detailed description of the invention]

産業上の利用分野 この発明は短波長記録に有用な金属薄膜型の磁
気記録媒体に関するものである。 従来例の構成とその問題点 従来より、磁気記録媒体は基板上に磁気記録層
として酸化鉄微粒子や合金微粒子をバインダ、添
加剤等と共に高分散させた塗料を塗布、乾燥させ
た、いわゆる塗布型のものが広く使用されてい
た。 しかしながら、近年、磁気記録はより高密度化
が望まれるようになり、Cr−Ni−O系の斜方蒸
着膜やCo−Cr等の垂直磁化膜等を磁気記録層と
するいわゆる金属薄膜型磁気記録媒体が注目さ
れ、研究開発が盛んになつた。ところが、このも
のはその電磁変換特性上の優位性が明らかになる
反面、実用耐久性において改良が望まれるもので
あることがはつきりしてきた。 この問題は、従来の塗布型磁気記録媒体と表面
の物性が変化した点と、短波長記録再生でのスペ
ーシングロスを低減化するため表面を平滑化した
点との相乗作用により、システムを構成するトラ
ンスポート系、シリンダ、磁気ヘツド等との摩擦
抵抗が大きく走行性能が悪いため、画質の劣化は
もちろん、磁性層がけずれて全く磁気記録媒体の
機能を失うことすらあつた。それゆえ、この点の
改良は実用化上必須の課題といえるものであつ
た。 そのため、従来の金属薄膜型磁気記録媒体であ
つては、第1図に示すように、非磁性基板1上に
強磁性金属薄膜2を設けたのち、表面の摩擦抵抗
を引下げるために、脂肪酸、脂肪酸エステル、脂
肪酸アミド、シリコーンオイル、動植物油の単独
または混合材料等の滑剤を強磁性金属膜2表面に
塗布して滑性被覆層3を形成することが行なわれ
ていた。 しかしながら、いずれの滑性被覆層3を用いて
も、初期の摩擦抵抗を引下げるのには効果がある
ものの、繰返し記録、再生を行なうと滑剤の効果
が薄れてくるとともに、高温高湿下でVTRの静
止画像を再生すると短時間で磁性層にすり傷が発
生する等の問題があり、充分な実用耐久性を具備
した金属薄膜型磁気記録媒体は得られていないの
が実情であつた。 発明の目的 この発明は充分な走行耐久性およびスチル耐久
性を有する金属薄膜型の磁気記録媒体を提供する
ことを目的とする。 発明の構成 この発明の磁気記録媒体は、非磁性基板上にこ
の基板と部分的に剥離状態にある強磁性金属薄膜
を設けたものである。 第2図はこの発明の磁気記録媒体の一例を示す
拡大断面図である。第2図において、1は非磁性
基板、2は強磁性金属薄膜、3は滑性被覆層であ
り、非磁性基板1と強磁性金属薄膜2との間には
部分的に金属薄膜2が剥離した剥離部4が形成さ
れる。 前記非磁性基板1としては、プラスチツクフイ
ルムまたはこのフイルム上に下地層を設けたもの
があげられる。プラスチツクフイルムとしては、
たとえばポリエチレンテレフタレート、ポリエチ
レンナフタレート、芳香族ポリアミド、ポリイミ
ド等が使用可能である。 また、強磁性金属薄膜2としては、たとえば
Co,Fe,Co−Ni,Co−Fe,Co−B,Co−Pt,
Co−Cu,Co−Cr,Co−Vまたはそれらの部分
酸化膜等の面内磁化膜、Co−Cr,Co−Ti,Co−
Mo,Co−W,Co−V,Co−Sm,Co−Ru,Co
−Mn,Co−Ni−Cr,Co−Cr−Rh等の垂直磁化
膜があげられる。非磁性基板1への強磁性金属薄
膜2の形成方法としては、たとえば真空蒸着法、
スパツタリング法、イオンプレーデイング法、C.
V.D.法、イオンビームデポジシヨン法、電気め
つき法、無電解めつき法等が使用可能である。 さらに、前記滑性被覆層3は必要に応じて使用
されるものであり、滑剤を強磁性金属薄膜2上に
塗布して形成することができる。滑剤としてはと
くにその種類が限定されるものではないが、たと
えば脂肪酸、脂肪酸の金属石けん、脂肪酸アミ
ド、脂肪酸エステル、鉱油、動植物油、シリコー
ンオイル、高級アルコール、フルオロカーボン等
の単体またはそれらの混合物が使用可能である。 非磁性基板1と強磁性金属薄膜2との間に部分
的に形成される剥離部4には、単に空気が入つた
空〓か、あるいは有機化合物等が混在した空〓が
形成される。かかる剥離部4が基板の表面全体に
占める割合は約1%から50%、好ましくは5%か
ら20%、より好ましくは5%から10%が適当であ
る。割合が1%より小なるときは耐久性能の向上
がみられず、従来例との差異が明確でない。ま
た、50%より大なるときは耐久性能が逆に悪くな
る。また1個の剥離部4の面積は約10-7cm2から
10-5cm、好ましくは10-7cm2から10-6cm2のオーダで
あるのが適当であるが、磁気ヘツド材質、形状等
により適宜変更しうるものであり、とくにその割
合が限定されるものではない。 このように剥離部4を設けることにより、磁気
記録媒体に応力緩和作用が働き、耐久性を向上さ
せると考えられる。具体的には一定温度で湿度を
広範囲(たとえば5〜95%RHの範囲)に変化さ
せても、殆ど摩擦抵抗の変化が起らず、またスチ
ル寿命が向上するという効果となつて現われるの
である。 実施例の説明 実施例 1 高さがせいぜい150Åで径が10μm以下の粒子
が表面に1万個/mm2で分散した平均粗さ80Åのポ
リエチレンテレフタレートフイルム(幅50cm、厚
さ10.5μm)の表面にステアリン酸を50Åの厚さ
で塗布したのち、張力6Kgで巻回し、50℃、60%
RHの雰囲気で3日間保存した。 ついで、前記フイルムの表面にCo−Ni(Ni含
量20重%)を酸素分圧2×10-5torrの真空中で最
小入射角30゜で斜め蒸着し、厚さ0.1μmの強磁性
金属薄膜を得た。このとき前記保存中にフイルム
表面に転写してステアリン酸により、金属薄膜は
剥離状態になつていた。形成された剥離部は平均
的に長円状でその長軸がフイルムの長手方向にあ
り、またその面積は6.5×10-6cm2で密度は3万
個/cm2であつた。 これを幅8mmのテープ状にスリツトした。これ
を試料1−Aとする。 また、前記強磁性金属薄膜上にステアリン酸亜
鉛の滑性被覆層を厚さ40Åで塗布し、幅8mmのテ
ープ状にスリツトした。これを試料1−Bとす
る。 実施例 2 高さが100Åで径が4μmの粒子が表面に4万
個/mm2で分散した平均粗さ50Åの芳香族ポリアミ
ドフイルム(幅50cm、厚さ8.5μm)の裏面にベヘ
ン酸を60Åの厚さで塗布したのち、張力6Kgで巻
回し、50℃80%RHの雰囲気下で3日間保存し
た。 ついで、前記フイルムの表面にCo−Cr(Cr含量
20重量%)を8×10-6torrの真空中で入射角を10゜
以内に限定して電子ビーム蒸着法により厚さ0.2μ
mの強磁性金属薄膜を得た。このとき、前記保存
中にフイルム表面に部分的に転写したベヘン酸に
よつて金属薄膜は剥離状態になつていた。形成さ
れた剥離部はその面積が4×10-6cm3で密度は6万
個/cm2であつた。 これを幅8mmのテープ状にスリツトした。これ
を試料2−Aとする。 また、前記強磁性金属薄膜上にステアリン酸ブ
チルの滑性被覆層を厚さ40Åで塗布し、幅8mmの
テープ状にスリツトした。これを試料2−Bとす
る。 比較例 1 ステアリン酸をフイルム裏面に塗布しなかつた
ほかは実施例1と同様にして表面に滑性被覆層を
設けた磁気テープを得た。これを試料1−Cとす
る。 比較例 2 ベヘン酸をフイルム裏面に塗布しなかつたほか
は実施例2と同様にして表面に滑性被覆層を設け
た磁気テープを得た。これを試料2−Cとする。 各実施例および比較例で得た各試料について、
走行耐久性およびスチル寿命を調べた。その結果
を次表に示す。なお、走行耐久性は初期値のS/N
を0dBとし、300回走行後の出力で示した。また、
スチル寿命は出力が初期値から−3dBに低下した
時間で示した。
INDUSTRIAL APPLICATION FIELD This invention relates to a metal thin film type magnetic recording medium useful for short wavelength recording. Conventional structure and its problems Traditionally, magnetic recording media have been of the so-called coating type, in which a paint in which iron oxide fine particles or alloy fine particles are highly dispersed together with a binder, additives, etc. is applied and dried as a magnetic recording layer on a substrate. were widely used. However, in recent years, there has been a demand for higher density magnetic recording, and so-called metal thin film magnetic Recording media attracted attention, and research and development became active. However, while it has become clear that this product has superior electromagnetic conversion characteristics, it has become clear that improvements in practical durability are desired. This problem was solved by the synergistic effect of the change in the physical properties of the surface compared to conventional coated magnetic recording media and the smoothing of the surface to reduce spacing loss during short wavelength recording and playback. Because of the large frictional resistance between the transport system, cylinder, magnetic head, etc., and poor running performance, not only did the image quality deteriorate, but the magnetic layer was even damaged, causing the magnetic recording medium to lose its functionality. Therefore, improvement in this point was an essential issue for practical use. Therefore, in conventional metal thin film magnetic recording media, as shown in FIG. 1, after a ferromagnetic metal thin film 2 is provided on a nonmagnetic substrate 1, a fatty acid The lubricant coating layer 3 has been formed by coating the surface of the ferromagnetic metal film 2 with a lubricant such as a fatty acid ester, a fatty acid amide, a silicone oil, or a mixture of animal and vegetable oils. However, although any type of lubricant coating layer 3 is effective in lowering the initial frictional resistance, repeated recording and playback will weaken the lubricant effect, and the lubricant will lose its effectiveness under high temperature and high humidity conditions. When playing still images from a VTR, there are problems such as scratches occurring in the magnetic layer in a short period of time, and the reality is that a metal thin film type magnetic recording medium with sufficient practical durability has not been obtained. OBJECTS OF THE INVENTION It is an object of the present invention to provide a metal thin film type magnetic recording medium having sufficient running durability and still durability. Structure of the Invention The magnetic recording medium of the present invention has a ferromagnetic metal thin film provided on a non-magnetic substrate and partially separated from the substrate. FIG. 2 is an enlarged sectional view showing an example of the magnetic recording medium of the present invention. In FIG. 2, 1 is a nonmagnetic substrate, 2 is a ferromagnetic metal thin film, and 3 is a slippery coating layer, and the metal thin film 2 is partially peeled off between the nonmagnetic substrate 1 and the ferromagnetic metal thin film 2. A peeled part 4 is formed. The non-magnetic substrate 1 may be a plastic film or a base layer provided on the film. As a plastic film,
For example, polyethylene terephthalate, polyethylene naphthalate, aromatic polyamide, polyimide, etc. can be used. Further, as the ferromagnetic metal thin film 2, for example,
Co, Fe, Co-Ni, Co-Fe, Co-B, Co-Pt,
In-plane magnetized films such as Co-Cu, Co-Cr, Co-V or their partially oxidized films, Co-Cr, Co-Ti, Co-
Mo, Co-W, Co-V, Co-Sm, Co-Ru, Co
-Mn, Co-Ni-Cr, Co-Cr-Rh, and other perpendicularly magnetized films. Examples of methods for forming the ferromagnetic metal thin film 2 on the nonmagnetic substrate 1 include vacuum evaporation,
Sputtering method, ion plating method, C.
VD method, ion beam deposition method, electroplating method, electroless plating method, etc. can be used. Furthermore, the slip coating layer 3 is used as required, and can be formed by coating the ferromagnetic metal thin film 2 with a lubricant. The type of lubricant is not particularly limited, but for example, fatty acids, fatty acid metal soaps, fatty acid amides, fatty acid esters, mineral oils, animal and vegetable oils, silicone oils, higher alcohols, fluorocarbons, etc. alone or mixtures thereof are used. It is possible. In the peeled portion 4 partially formed between the nonmagnetic substrate 1 and the ferromagnetic metal thin film 2, a void containing air or a void containing an organic compound or the like is formed. The ratio of the peeled portion 4 to the entire surface of the substrate is approximately 1% to 50%, preferably 5% to 20%, and more preferably 5% to 10%. When the ratio is less than 1%, no improvement in durability is observed, and the difference from the conventional example is not clear. Moreover, when it is greater than 50%, the durability performance deteriorates. Also, the area of one peeled part 4 is approximately 10 -7 cm 2
A suitable value is 10 -5 cm, preferably on the order of 10 -7 cm 2 to 10 -6 cm 2 , but it can be changed as appropriate depending on the material, shape, etc. of the magnetic head, and in particular, the ratio is limited. It's not something you can do. It is thought that by providing the peeling portion 4 in this way, a stress relaxing effect acts on the magnetic recording medium, improving durability. Specifically, even if the humidity is varied over a wide range (for example, from 5 to 95% RH) at a constant temperature, there is almost no change in frictional resistance, and the still life is improved. . Description of Examples Example 1 Surface of a polyethylene terephthalate film (width 50 cm, thickness 10.5 μm) with an average roughness of 80 Å, on which particles with a height of at most 150 Å and a diameter of 10 μm or less are dispersed at a rate of 10,000 particles/mm 2 After applying stearic acid to a thickness of 50 Å, it was wound with a tension of 6 kg and heated at 50°C, 60%.
It was stored in an RH atmosphere for 3 days. Next, Co-Ni (Ni content: 20% by weight) was obliquely deposited on the surface of the film at a minimum incident angle of 30° in a vacuum with an oxygen partial pressure of 2×10 -5 torr to form a ferromagnetic metal thin film with a thickness of 0.1 μm. I got it. At this time, the metal thin film had been transferred to the film surface during the storage and had become peeled off due to stearic acid. The formed peeled portions had an average oval shape with their major axes in the longitudinal direction of the film, and had an area of 6.5×10 −6 cm 2 and a density of 30,000 pieces/cm 2 . This was slit into a tape shape with a width of 8 mm. This is designated as sample 1-A. Further, a slip coating layer of zinc stearate was applied to a thickness of 40 Å on the ferromagnetic metal thin film, and the film was slit into a tape having a width of 8 mm. This is designated as sample 1-B. Example 2 60 Å of behenic acid was applied to the back surface of an aromatic polyamide film (width 50 cm, thickness 8.5 µm) with an average roughness of 50 Å, in which 40,000 particles/mm 2 with a height of 100 Å and a diameter of 4 μm were dispersed on the surface. After coating the film to a thickness of , it was wound with a tension of 6 kg and stored in an atmosphere of 50°C and 80% RH for 3 days. Next, Co-Cr (Cr content:
20% by weight) to a thickness of 0.2μ by electron beam evaporation in a vacuum of 8×10 -6 torr with an incident angle limited to within 10°.
A ferromagnetic metal thin film of m was obtained. At this time, the metal thin film was in a peeled state due to behenic acid partially transferred to the film surface during the storage. The area of the formed peeled portion was 4×10 −6 cm 3 and the density was 60,000 pieces/cm 2 . This was slit into a tape shape with a width of 8 mm. This is designated as sample 2-A. Further, a slip coating layer of butyl stearate was applied to a thickness of 40 Å on the ferromagnetic metal thin film, and the film was slit into a tape having a width of 8 mm. This is designated as sample 2-B. Comparative Example 1 A magnetic tape having a slip coating layer on the surface was obtained in the same manner as in Example 1 except that stearic acid was not applied to the back surface of the film. This is designated as sample 1-C. Comparative Example 2 A magnetic tape having a slip coating layer on the surface was obtained in the same manner as in Example 2, except that behenic acid was not applied to the back surface of the film. This is designated as sample 2-C. For each sample obtained in each example and comparative example,
Running durability and still life were investigated. The results are shown in the table below. In addition, running durability is the initial value S/N
is set to 0dB, and the output is shown after 300 runs. Also,
The still life was expressed as the time required for the output to drop to -3 dB from the initial value.

【表】【table】

【表】 表から、実施例1および2で得た各試料は走行
耐久性にすぐれ、スチル寿命も飛躍的に向上して
いるのがわかる。その結果、繰返し走行による画
質の変化は殆どなく、すぐれた短波長出力を実用
にでき、さらにそのスチル寿命によつてすぐれた
スチル再生を行なうことができた。 発明の効果 この発明の磁気記録媒体は、走行耐久性および
スチル耐久性にすぐれているという効果がある。
[Table] From the table, it can be seen that each sample obtained in Examples 1 and 2 has excellent running durability and has a dramatically improved still life. As a result, there was almost no change in image quality due to repeated running, excellent short-wavelength output could be put to practical use, and further, excellent still reproduction could be performed due to the still life. Effects of the Invention The magnetic recording medium of the present invention has an effect of being excellent in running durability and still durability.

【図面の簡単な説明】[Brief explanation of the drawing]

第1図は従来の金属薄膜型磁気記録媒体の拡大
断面図、第2図はこの発明の磁気記録媒体の一例
を示す拡大断面図である。 1…非磁性基板、2…強磁性金属薄膜、4…剥
離部。
FIG. 1 is an enlarged sectional view of a conventional metal thin film type magnetic recording medium, and FIG. 2 is an enlarged sectional view showing an example of the magnetic recording medium of the present invention. DESCRIPTION OF SYMBOLS 1...Nonmagnetic substrate, 2...Ferromagnetic metal thin film, 4...Peeling part.

Claims (1)

【特許請求の範囲】[Claims] 1 非磁性基板と、この基板上に設けられ基板と
部分的に剥離状態にある強磁性金属薄膜とを備え
た磁気記録媒体。
1. A magnetic recording medium comprising a non-magnetic substrate and a ferromagnetic metal thin film provided on the substrate and partially separated from the substrate.
JP58083359A 1983-05-12 1983-05-12 magnetic recording medium Granted JPS59207424A (en)