JPH0471973B2 - - Google Patents
Info
- Publication number
- JPH0471973B2 JPH0471973B2 JP62162419A JP16241987A JPH0471973B2 JP H0471973 B2 JPH0471973 B2 JP H0471973B2 JP 62162419 A JP62162419 A JP 62162419A JP 16241987 A JP16241987 A JP 16241987A JP H0471973 B2 JPH0471973 B2 JP H0471973B2
- Authority
- JP
- Japan
- Prior art keywords
- slurry
- preform
- inorganic
- sic
- adjusted
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Lifetime
Description
〔産業上の利用分野〕
本発明は、金属やプラスチツクなどのマトリツ
クス物質を溶浸して繊維強化複合材を製造する際
に、その繊維質骨格として用いるSiCウイスカー
プリフオームの製造方法に関する。
〔従来の技術〕
ウイスカーなどの短繊維状物質を強化材として
繊維強化複合材を製造するための有効な手段に、
所定形状に成形したウイスカープリフオームをモ
ールド内に設置し、このプリフオームに液状のマ
トリツクス物質を圧入固化させる方法がある。こ
の方法によつて得られる複合材の特性は、繊維質
骨格となるウイスカープリフオームの組織構造、
特にその均質性に大きく影響される。
均質組織のウイスカープリフオームの製造方法
としてはいろいろな方法が提案されているが、そ
の多くはウイスカーを水または有機溶媒に分散さ
せた分散液を加圧過もしくは吸引過乾燥する
分散過法を基本としている。
しかしながら、SiCウイスカーは、直径0.1〜1μ
m、長さが30〜100μm程度の微細短繊維状の物
質であり、これらが複雑に絡み合つて凝集してい
るために完全に解きほぐすことは容易でない。し
たがつて、均質な分散液を作製することが難し
く、また過過程においても再凝集し易い。その
結果、得られるプリフオームの組織構造も不均質
化して、ラミネートや斑などを生じ易い欠点があ
る。更に分散液の濃度も、相対的に高濃度に設定
すると再凝集が促進されるため、比較的に低濃度
にしなければならず、一連の処理過程において大
量の液体の処理が必要となり、生産が非能率とな
る。また、この分散過法は、大型のプリフオー
ムや複雑形状のプリフオームを得難い問題点もあ
る。
〔発明が解決しようとする問題点〕
本発明は、上記問題点を解消して、均質に高分
散した高濃度の泥漿を用いて、均質組織構造を有
するプリフオームを能率よく製造する方法を提案
するものである。
〔問題点を解決するための手段〕
すなわち、本発明はPH11〜12に調整した無機質
解膠剤水溶液にSiCウイスカーを高濃度に混合し
たのち混練解膠して均質な泥漿とし、該泥漿を鋳
型に鋳混むことを特徴とするSiCウイスカープリ
フオームの製造方法である。
SiCウイスカーは微細形態を有し、セミコロイ
ド的挙動を示し、その分散性は分散媒界面におけ
る電気二重層に大きく影響される。すなわち分散
液のPHに依存する処が大きい。
本発明は、絡み合つたSiCウイスカーの分散を
促し、安定な分散状態を維持するために、無機質
解膠剤を使用し、高濃度、安定な泥漿を得るもの
である。無機質解膠剤は、プリフオーム中に残留
して繊維強化複合材を製造した場合に特性劣化を
生じる場合がある。したがつて、その使用量は少
ない程好ましい。本発明はこの観点からPHを11〜
12に設定するものである。更にPHが12を上回つて
も泥漿の分散および安定化効果の著しい向上が認
められないためである。泥漿はSiCウイスカー濃
度を20wt%以上に設定することができるが高濃
度化とともに粘度上昇が大きくなるので、40wt
%以下に抑えることが好ましい。この高濃度の泥
漿は、混練機により強力な剪断力を利用して混練
解膠することにより、均質、安定な泥漿を得るこ
とができ、単なる攪拌混合では好ましい泥漿を得
ることが困難である。
無機質解膠剤としては、種々のものが使用でき
るが、SiCウイスカーに対する解膠機能の大きい
苛性ソーダ、水ガラス、アルミン酸ソーダなどが
好ましく用いられる。
また、無機質解膠剤は熱処理などで除去するこ
とができれば繊維強化複合材中への残留が防止で
きるので好ましい。そのために予めアンモニア水
でPHを10〜11に調整し、これに無機質解膠剤を添
加してPHを11〜12に調整すればアンモニアは加熱
処理で容易に揮散するので、残留する無機質解膠
剤を少量に抑制することができる。
このようにして得られた泥漿は、泥漿鋳込み法
により、石膏型などの鋳型に注入して泥漿を着肉
させることにより、均質組成のプリフオーム成形
体を得ることができる。
〔作用〕
上記構成により、本発明は無機質解膠剤水溶液
中に、SiCウイスカーを高濃度に混合したのち強
力な剪断力により混練処理するので、ウイスカー
が効果的に解膠され、また安定な分散状態を保持
した泥漿を効率よく形成することができる。
〔実施例〕
実施例 1
苛性ソーダを純水に溶解してPH11.8の苛性ソー
ダ水溶液2600mlを調製し、この中に直径0.5〜1μ
m、長さ30〜100μmのSiCウイスカーを加えて
25wt%の混合物を調製した。この混合物をウエ
ルナー型混練機で30分間混練して均質な泥漿を得
た。この泥漿の粘度は約1000cpであつた。次い
で内径80mm、高さ150mmの円筒形の石膏型に注入
して着肉させた後、石膏型から取り外し、直径
79.9mm、高さ150mmの円柱状のプリフオームを作
製した。
このプリフオームから測定試片を切出した。試
片は中心部から30×30mm、高さ150mmの角柱を切
出し、高さ方向から等分の間隔で切断して、30mm
角の立方体試片5ケを作製した。
この各試片について、Vfおよび圧縮強度を測
定した。圧縮強度は試片が座屈破壊または厚さが
10%以上の変形を生じる時の荷重で示した。
これらの結果を表−1に示した。
比較のために純水2600ml中にSiCウイスカーを
加えて、25wt%の混合物とし、実施例と同じ方
法で捏合したがウイスカーの凝集塊が生成して、
安定な分散状態の泥漿を得ることができず、プリ
フオームの作製は不可能であつた。なお、翼型攪
拌機を用いて、純水中にSiCウイスカーを12wt%
の割合に攪拌混合し、過乾燥する分散過法に
より作製したプリフオームの特性値を表−1に併
記した。
[Industrial Application Field] The present invention relates to a method for manufacturing a SiC whisker preform used as a fibrous skeleton when manufacturing a fiber-reinforced composite material by infiltrating a matrix material such as metal or plastic. [Prior Art] An effective means for producing fiber-reinforced composite materials using short fibrous substances such as whiskers as reinforcing materials.
There is a method in which a whisker preform molded into a predetermined shape is placed in a mold, and a liquid matrix material is press-fitted into the preform and solidified. The characteristics of the composite material obtained by this method are the structure of the whisker preform, which is the fibrous skeleton;
In particular, it is greatly influenced by its homogeneity. Various methods have been proposed for producing whisker preforms with a homogeneous structure, but most of them are based on the dispersion method, in which a dispersion of whiskers in water or an organic solvent is dried under pressure or suction. It is said that However, SiC whiskers have a diameter of 0.1 to 1μ
It is a short, fine fiber-like substance with a length of about 30 to 100 μm, and it is difficult to completely disentangle it because it is intricately intertwined and aggregated. Therefore, it is difficult to prepare a homogeneous dispersion liquid, and it is also easy to re-agglomerate during the process. As a result, the tissue structure of the obtained preform becomes non-uniform, resulting in the disadvantage that lamination and spots are likely to occur. Furthermore, if the concentration of the dispersion liquid is set to a relatively high concentration, reaggregation will be promoted, so it must be kept at a relatively low concentration, and a large amount of liquid must be treated in a series of processing steps, which reduces production. It becomes inefficient. Further, this dispersion method has the problem that it is difficult to obtain a large preform or a preform with a complicated shape. [Problems to be Solved by the Invention] The present invention solves the above-mentioned problems and proposes a method for efficiently manufacturing a preform having a homogeneous texture using a highly concentrated homogeneously dispersed slurry. It is something. [Means for solving the problem] That is, the present invention mixes SiC whiskers at a high concentration in an aqueous inorganic peptizer solution adjusted to pH 11 to 12, then kneads and peptizes it to form a homogeneous slurry, and uses the slurry as a mold. This is a method for manufacturing a SiC whisker preform, which is characterized by mixing the SiC whisker preform with the SiC whisker preform. SiC whiskers have a fine morphology and exhibit semicolloidal behavior, and their dispersibility is greatly influenced by the electric double layer at the dispersion medium interface. In other words, it largely depends on the pH of the dispersion. The present invention uses an inorganic deflocculant to promote the dispersion of entangled SiC whiskers and maintain a stable dispersion state, thereby obtaining a highly concentrated and stable slurry. An inorganic deflocculant may remain in a preform and cause property deterioration when a fiber-reinforced composite material is manufactured. Therefore, the smaller the amount used, the better. From this point of view, the present invention improves the pH from 11 to
It is set to 12. Furthermore, even if the pH exceeds 12, no significant improvement in the dispersion and stabilization effect of the slurry is observed. The SiC whisker concentration of the slurry can be set to 20wt% or more, but as the concentration increases, the viscosity increases, so 40wt% or more is required.
% or less. A homogeneous and stable slurry can be obtained by kneading and peptizing this highly concentrated slurry using a strong shearing force in a kneader, and it is difficult to obtain a desirable slurry by simply stirring and mixing. Various inorganic peptizers can be used, but caustic soda, water glass, sodium aluminate, and the like, which have a large peptizing function against SiC whiskers, are preferably used. Further, it is preferable that the inorganic deflocculant can be removed by heat treatment or the like, since this can prevent it from remaining in the fiber-reinforced composite material. For this purpose, adjust the pH to 10-11 with ammonia water in advance, and then add an inorganic peptizer to adjust the pH to 11-12.The ammonia will easily volatilize during heat treatment, so the remaining inorganic peptizer will be removed. agent can be suppressed to a small amount. The slurry thus obtained is injected into a mold such as a plaster mold by a slurry casting method to form a preform molded body having a homogeneous composition. [Function] With the above configuration, the present invention mixes SiC whiskers at a high concentration in an aqueous solution of an inorganic deflocculant and then kneads them using strong shearing force, so that the whiskers are effectively deflocculated and stable dispersion is achieved. A slurry that maintains its state can be efficiently formed. [Example] Example 1 Dissolve caustic soda in pure water to prepare 2600 ml of caustic soda aqueous solution with a pH of 11.8.
m, by adding SiC whiskers with a length of 30 to 100 μm.
A 25wt% mixture was prepared. This mixture was kneaded for 30 minutes using a Werner type kneader to obtain a homogeneous slurry. The viscosity of this slurry was approximately 1000 cp. Next, after pouring it into a cylindrical plaster mold with an inner diameter of 80 mm and a height of 150 mm, it was removed from the plaster mold and the diameter
A cylindrical preform with a diameter of 79.9 mm and a height of 150 mm was manufactured. A measurement specimen was cut from this preform. For the specimen, cut out a 30 x 30 mm square column and 150 mm height from the center, cut it at equal intervals from the height direction, and cut it into 30 mm pieces.
Five corner cube specimens were prepared. Vf and compressive strength were measured for each specimen. Compressive strength is determined by whether the specimen undergoes buckling failure or thickness
It is expressed as the load that causes deformation of 10% or more. These results are shown in Table-1. For comparison, SiC whiskers were added to 2600 ml of pure water to make a 25 wt% mixture and kneaded in the same manner as in the example, but whisker aggregates were formed.
It was not possible to obtain a slurry in a stable dispersed state, and it was impossible to produce a preform. In addition, 12wt% of SiC whiskers were added to pure water using a blade-type stirrer.
Table 1 also shows the characteristic values of the preform produced by the dispersion filtration method in which the materials are stirred and mixed at a ratio of 1, and then overdried.
上記説明で明らかなように、本発明により高濃
度かつ均質で安定な泥漿を得ることができる。こ
の泥漿を、泥漿鋳込み法により製造したプリフオ
ームも均質性ならびに強度が高く、極めて能率的
にプリフオームの製造が可能となる。また、形状
が複雑なプリフオームや大型のプリフオームの成
形も容易である。したがつて優れた強度特性を有
する繊維強化複合材を能率よく製造することが可
能となる。
As is clear from the above description, a highly concentrated, homogeneous and stable slurry can be obtained according to the present invention. A preform manufactured from this slurry by the slurry casting method also has high homogeneity and strength, and can be manufactured extremely efficiently. Furthermore, it is easy to mold preforms with complicated shapes or large preforms. Therefore, it becomes possible to efficiently produce a fiber-reinforced composite material having excellent strength characteristics.
Claims (1)
SiCウイスカーを20〜40wt%の範囲で混合したの
ち強力な剪断力下に混練解膠して均質な泥漿と
し、該泥漿を石膏鋳型に鋳込むことを特徴とする
SiCウイスカープリフオームの製造方法。 2 予めPH10〜11に調整したアンモニア水溶液に
無機質解膠剤を加えてPH11〜12に調整する特許請
求野範囲第1項記載のSiCウイスカープリフオー
ムの製造方法。 3 無機質解膠剤が苛性ソーダ、水ガラス、アル
ミン酸ソーダである特許請求の範囲第1項記載の
SiCウイスカープリフオームの製造方法。[Claims] 1. An inorganic deflocculant aqueous solution adjusted to PH11 to 12.
It is characterized by mixing SiC whiskers in a range of 20 to 40 wt%, kneading and peptizing the mixture under strong shearing force to form a homogeneous slurry, and casting the slurry into a plaster mold.
Method for manufacturing SiC whisker preform. 2. The method for producing a SiC whisker preform according to claim 1, wherein the pH is adjusted to 11 to 12 by adding an inorganic peptizer to an ammonia aqueous solution that has been adjusted to PH 10 to 11 in advance. 3. Claim 1, wherein the inorganic deflocculant is caustic soda, water glass, or sodium aluminate.
Method for manufacturing SiC whisker preform.