JPH06101032A - Sputtering target - Google Patents

Sputtering target

Info

Publication number
JPH06101032A
JPH06101032A JP24772892A JP24772892A JPH06101032A JP H06101032 A JPH06101032 A JP H06101032A JP 24772892 A JP24772892 A JP 24772892A JP 24772892 A JP24772892 A JP 24772892A JP H06101032 A JPH06101032 A JP H06101032A
Authority
JP
Japan
Prior art keywords
sputtering
composition
thin film
sputtering target
oxide
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
JP24772892A
Other languages
Japanese (ja)
Inventor
Yuji Watanabe
雄二 渡辺
Gentaro Obayashi
元太郎 大林
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toray Industries Inc
Original Assignee
Toray Industries Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toray Industries Inc filed Critical Toray Industries Inc
Priority to JP24772892A priority Critical patent/JPH06101032A/en
Publication of JPH06101032A publication Critical patent/JPH06101032A/en
Ceased legal-status Critical Current

Abstract

(57)【要約】 【構成】本発明は、少なくとも、カルコゲン化合物、酸
化物および炭素(C)を含むスパッタリングターゲット
であって、該ターゲットは、酸化物−炭素複合体と、カ
ルコゲン化合物とを成型してなるものであることを特徴
とするスパッタリングターゲットに関する。 【効果】本発明のスパッタリングターゲットをスパッタ
リングして薄膜を形成する場合、形成された薄膜の組成
がターゲットの組成と極めて良く一致し、所望の組成の
薄膜が容易に形成できる。さらに、長期にわたるスパッ
タリングを行っても、ターゲット表面の組成が変化せず
に、形成される薄膜の組成もほとんど変化しない。
(57) [Summary] [Constitution] The present invention is a sputtering target containing at least a chalcogen compound, an oxide and carbon (C), the target being formed by molding an oxide-carbon composite and a chalcogen compound. And a sputtering target. [Effect] When a thin film is formed by sputtering the sputtering target of the present invention, the composition of the formed thin film matches the composition of the target very well, and a thin film having a desired composition can be easily formed. Furthermore, even if sputtering is performed for a long period of time, the composition of the target surface does not change, and the composition of the formed thin film hardly changes.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、真空薄膜形成により誘
電体薄膜を形成する際に用いられるスパッタリングター
ゲットに関するものである。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a sputtering target used for forming a dielectric thin film by vacuum thin film formation.

【0002】[0002]

【従来の技術】カルコゲン化合物と酸化物と炭素よりな
る誘電体膜は、アモルファスあるいはアモルファスライ
クな膜で、高温熱安定性に優れており、さらに膜内部応
力が小さい等の優れた特性を有している。そのため、光
学薄膜、保護膜、絶縁膜などの広い用途があり、特に光
記録媒体の誘電体層として最適である。相変化書換形光
記録媒体の誘電体層として、カルコゲン化合物と酸化物
と炭素よりなる誘電体を用いると、記録特性が優れてい
るばかりでなく、長期信頼性、記録繰り返し性に優れた
光記録媒体が得られる。
2. Description of the Related Art A dielectric film composed of a chalcogen compound, an oxide, and carbon is an amorphous or amorphous-like film, which has excellent high-temperature thermal stability and further has excellent properties such as a small internal stress in the film. ing. Therefore, it has a wide range of applications such as an optical thin film, a protective film, and an insulating film, and is most suitable as a dielectric layer of an optical recording medium. When a dielectric composed of a chalcogen compound, an oxide, and carbon is used as the dielectric layer of a phase-change rewritable optical recording medium, not only excellent recording characteristics but also excellent long-term reliability and recording repeatability are achieved. The medium is obtained.

【0003】カルコゲン化合物と酸化物と炭素よりなる
誘電体膜をスパッタリングにより作成する場合、それぞ
れの成分のスパッタリングターゲットを2元同時スパッ
タリング、あるいは3元同時スパッタリングすることに
より所望の組成の薄膜を形成していた。あるいは、カル
コゲン化合物、酸化物、炭素を、単独の状態で、所望の
薄膜の組成比と同じ比でそれぞれの粉末を混合した後
に、ホットプレス等により所望の形状に成型して作製し
たスパッタリングターゲットを用いて、スパッタリング
を行っていた。
When a dielectric film made of a chalcogen compound, an oxide and carbon is formed by sputtering, a sputtering target of each component is simultaneously sputtered with two or three elements to form a thin film having a desired composition. Was there. Alternatively, the chalcogen compound, the oxide, the carbon, in a single state, after mixing each powder in the same ratio as the composition ratio of the desired thin film, the sputtering target formed by molding into a desired shape by hot pressing or the like. It was used to perform sputtering.

【0004】2元同時スパッタリング、あるいは3元同
時スパッタリングによる薄膜の作成は、生産レベルのス
パッタリングでは薄膜の組成の安定性の面で問題があ
り、さらにスパッタリング装置上からも、多くのスパッ
タリングターゲット、カソード、電源などが必要とな
る。そのため、1つのスパッタリングターゲットから所
望の組成の薄膜が形成されることが望ましい。
The production of a thin film by two-source simultaneous sputtering or three-source simultaneous sputtering has a problem in the stability of the composition of the thin film in the production level sputtering, and many sputtering targets and cathodes are also available from the sputtering apparatus. , Power supply, etc. are required. Therefore, it is desirable that a thin film having a desired composition be formed from one sputtering target.

【0005】ところで、一般に高いスパッタリングレー
トを持つカルコゲン化合物に比較して、炭素は極めてス
パッタリングレートが低い。そこで、カルコゲン化合物
と酸化物と炭素からなるスパッタリングターゲットをス
ッパッタリングして薄膜を形成する場合、薄膜において
は、カルコゲン化合物と酸化物の相対比はスパッタリン
グターゲット組成の相対比と同一になるが、炭素の組成
比はスパッタリングターゲット組成比に対して極めて少
なくなってしまう場合がある。また、このスパッタリン
グレートの大きな差のために、スパッタリングターゲッ
ト表面の組成が、本来の組成に対して経時的に変化して
炭素の比が大きくなるために、形成される薄膜の組成が
経時的に変化してしまう。
By the way, carbon generally has an extremely low sputtering rate as compared with a chalcogen compound having a high sputtering rate. Therefore, when forming a thin film by sputtering a sputtering target consisting of a chalcogen compound, an oxide and carbon, in the thin film, the relative ratio of the chalcogen compound and the oxide is the same as the relative ratio of the sputtering target composition, The composition ratio of carbon may be extremely smaller than the composition ratio of the sputtering target. Further, due to the large difference in the sputtering rate, the composition of the sputtering target surface changes with time with respect to the original composition and the ratio of carbon increases, so that the composition of the formed thin film changes with time. It will change.

【0006】[0006]

【発明が解決しようとする課題】したがって、本発明の
目的は、カルコゲン化合物と酸化物と炭素からなるスパ
ッタリングターゲットをスパッタリングして薄膜を形成
する場合、形成された薄膜の組成がターゲットの組成と
一致するスパッタリングターゲットを提供することにあ
る。
Therefore, when a thin film is formed by sputtering a sputtering target composed of a chalcogen compound, an oxide and carbon, the composition of the formed thin film is the same as the composition of the target. To provide a sputtering target.

【0007】本発明の別の目的は、長期にわたるスパッ
タリングを行っても、スパッタリングターゲット表面の
組成が変化せず、形成される薄膜の組成も変化しないス
パッタリングターゲットを提供することにある。
Another object of the present invention is to provide a sputtering target in which the composition of the surface of the sputtering target does not change and the composition of the thin film to be formed does not change even after performing sputtering for a long time.

【0008】[0008]

【課題を解決するための手段】かかる本発明の目的は、
少なくとも、カルコゲン化合物、酸化物および炭素
(C)を含むスパッタリングターゲットであって、該タ
ーゲットは、酸化物−炭素複合体と、カルコゲン化合物
とを成型してなるものであることを特徴とするスパッタ
リングターゲットにより達成される。
The object of the present invention is as follows.
A sputtering target containing at least a chalcogen compound, an oxide and carbon (C), wherein the target is formed by molding an oxide-carbon composite and a chalcogen compound. Achieved by

【0009】本発明におけるカルコゲン化合物として
は、硫化物、セレン化物、テルル化物などを言う。例え
ば、ZnS、ZnSe、ZnTe、PbS、PbSe、
PbTeなどの硫化物、セレン化物、テルル化物を挙げ
ることができるが、これらに限定されない。これらの中
で特に好ましいものは、ZnS、ZnSe、ZnTeで
ある。
The chalcogen compound in the present invention includes sulfides, selenides, tellurides and the like. For example, ZnS, ZnSe, ZnTe, PbS, PbSe,
Examples thereof include, but are not limited to, sulfides such as PbTe, selenides, and tellurides. Among these, ZnS, ZnSe, and ZnTe are particularly preferable.

【0010】本発明における酸化物としては、Si、A
l、Ti、Ta、Geなどの酸化物を挙げることができ
るが、これらに限定されない。これらの中で特に好まし
いものは、Si、Al、Tiの酸化物である。
The oxides used in the present invention include Si and A.
Examples thereof include oxides such as 1, Ti, Ta, and Ge, but are not limited thereto. Of these, particularly preferred are oxides of Si, Al, and Ti.

【0011】本発明における酸化物−炭素複合体として
は、元素Mの酸化物−炭素複合体を仮定した場合、例え
ば、M−O結合とM−C結合が共に認められる複合体で
あり、これらの結合は、赤外線吸収スペクトルなどで確
認することができる。
Assuming an oxide-carbon composite of the element M, the oxide-carbon composite in the present invention is, for example, a composite in which both an MO bond and an MC bond are recognized. The binding of can be confirmed by an infrared absorption spectrum or the like.

【0012】酸化物−炭素の複合体の作成方法として
は、特に限定されない。例えば、Si酸化物−C複合体
の場合、多孔質石英ガラスをメタンガス雰囲気で100
0℃程度で熱処理することにより、炭素/二酸化珪素の
モル比が0.5〜4.0程度の範囲の二酸化珪素−C複
合体を作成することができる。また、ポリカルボシラン
を1000℃〜1200℃で熱処理することにより、S
i−O−C複合体を作成することができる。さらに、ポ
リチタノカルボシランを熱処理することによりSi−T
i−O−C複合体を作成することができる。酸化物−炭
素複合体の中で、特に好ましいものは、Si−O−C複
合体である。
The method for producing the oxide-carbon composite is not particularly limited. For example, in the case of a Si oxide-C composite, porous quartz glass is used in a methane gas atmosphere at 100
By heat treatment at about 0 ° C., a silicon dioxide-C composite having a carbon / silicon dioxide molar ratio in the range of about 0.5 to 4.0 can be prepared. Further, by heat-treating polycarbosilane at 1000 ° C to 1200 ° C, S
An i-O-C complex can be made. Furthermore, by heat-treating polytitanocarbosilane, Si-T
An i-O-C complex can be made. Among the oxide-carbon composites, the Si-O-C composite is particularly preferable.

【0013】カルコゲン化合物と酸化物と炭素(C)か
らなるスパッタリングターゲットの組成としては、特に
限定されず、作成される薄膜の特性から要求される組成
とすることができるが、炭素/酸化物のモル比は5以下
であることが好ましい。炭素/酸化物のモル比が5を越
えると、酸化物−炭素複合体を作成することが容易でな
くなる場合がある。
The composition of the sputtering target composed of the chalcogen compound, the oxide and the carbon (C) is not particularly limited and may be a composition required from the characteristics of the thin film to be produced. The molar ratio is preferably 5 or less. When the carbon / oxide molar ratio exceeds 5, it may be difficult to prepare an oxide-carbon composite.

【0014】酸化物−炭素複合体とカルコゲン化合物よ
りスパッタリングターゲットを成型する方法としては、
例えばホットプレス、冷間静水圧プレス等の公知の方法
を用いることができる。スパッタリングターゲットの形
状としては、使用するスパッタリング装置によって選択
することができ、直径3〜8インチ程度の円形、または
(4〜6インチ)×(5〜20インチ)程度の方形など
が一般的である。スパッタリングターゲットの厚さとし
ては、通常、3〜20mm程度である。該スパッタリン
グターゲットはスパッタリング中の熱を効果的に放熱す
るために、バッキングプレートにボンディングして水冷
して使用することが好ましい。
As a method for molding a sputtering target from an oxide-carbon composite and a chalcogen compound,
For example, known methods such as hot pressing and cold isostatic pressing can be used. The shape of the sputtering target can be selected depending on the sputtering apparatus used, and is generally a circle having a diameter of about 3 to 8 inches, or a square of (4 to 6 inches) × (5 to 20 inches). . The thickness of the sputtering target is usually about 3 to 20 mm. In order to effectively dissipate heat during sputtering, it is preferable to bond the sputtering target to a backing plate and water-cool it for use.

【0015】[0015]

【実施例】以下、本発明を実施例にもとづいて説明する
が、本発明はこれらに限定されない。本発明のスパッタ
リングターゲットおよびこれを用いて作成した薄膜の組
成は、ICP発光分光分析法、管状電気抵抗加熱炉−赤
外線吸収法、ラザフォード後方散乱分光法(RBS)を
併用して確認した。
EXAMPLES The present invention will now be described based on examples, but the present invention is not limited to these. The composition of the sputtering target of the present invention and the thin film formed by using the sputtering target was confirmed by using ICP emission spectroscopy, tubular electric resistance heating furnace-infrared absorption method, and Rutherford backscattering spectroscopy (RBS) in combination.

【0016】実施例1 かさ密度0.4g/cm3 、比表面積10m2 /g、平
均粒子径0.3μmの多孔質合成石英ガラスを、メタン
ガス100%の雰囲気下で1000℃、1時間処理し、
炭素/二酸化珪素のモル比が2.0である二酸化珪素−
炭素複合体を作成した。ZnS粉末と二酸化珪素−炭素
複合体を、ZnS70モル%、二酸化珪素−炭素複合体
30モル%(SiO2 10モル%/C20モル%)の混
合比で十分に混合した。この混合粉末をホットプレスを
用いて成型後、直径4インチ、厚さ5mmの円盤状に整
形して本発明のスパッタリングターゲットを作成した。
Example 1 Porous synthetic quartz glass having a bulk density of 0.4 g / cm 3 , a specific surface area of 10 m 2 / g and an average particle size of 0.3 μm was treated at 1000 ° C. for 1 hour in an atmosphere of 100% methane gas. ,
Silicon dioxide having a carbon / silicon dioxide molar ratio of 2.0
A carbon composite was created. Carbon composites, ZnS70 mol%, silicon dioxide - - ZnS powder and silicon dioxide were mixed thoroughly in a mixing ratio of the carbon composite material 30 mol% (SiO 2 10 mol% / C20 mole%). This mixed powder was molded using a hot press and then shaped into a disk having a diameter of 4 inches and a thickness of 5 mm to prepare a sputtering target of the present invention.

【0017】このスパッタリングターゲットを無酸素銅
製のバッキングプレートにインジウム合金を用いてボン
ディングしたのち、スパッタリング装置にセットした。
スパッタリング装置は、基板−スパッタリングターゲッ
ト間距離が100mm、スパッタリング薄膜の組成、膜
厚を均一にするための基板自公転機構を有している。基
板としてポリカーボネート板およびSiウエハーを用い
た。スパッタリングチャンバー内部を1.0×10-4P
aまで真空排気したのち、Arガスを5.0×10-1P
aとなるように導入した。RFマグネトロンスパッタリ
ング法により、投入電力500Wでスパッタリングを行
い、基板上にZnS−Si−O−C薄膜を500nm形
成した。
This sputtering target was bonded to an oxygen-free copper backing plate using an indium alloy and then set in a sputtering apparatus.
The sputtering apparatus has a substrate-sputtering target distance of 100 mm and a substrate rotation / revolution mechanism for making the composition and film thickness of a sputtering thin film uniform. A polycarbonate plate and a Si wafer were used as the substrate. 1.0 x 10 -4 P inside the sputtering chamber
After evacuation to a, Ar gas is 5.0 × 10 -1 P
It was introduced so as to be a. Sputtering was performed with an input power of 500 W by an RF magnetron sputtering method to form a ZnS-Si-O-C thin film of 500 nm on the substrate.

【0018】形成された薄膜の組成は、ZnS70.3
モル%、SiO2 9.9モル%、C19.8モル%であ
り、スパッタリングターゲット組成と極めてよく一致し
ていた。さらに、同一条件でスパッタリングを繰り返し
ても、薄膜の組成はほとんど変動しなかった。
The composition of the formed thin film is ZnS70.3.
It was mol%, SiO 2 9.9 mol%, and C 19.8 mol%, which were in very good agreement with the sputtering target composition. Further, even if the sputtering was repeated under the same conditions, the composition of the thin film hardly changed.

【0019】実施例2 実施例1と同一の多孔質合成石英ガラスを、メタンガス
100%の雰囲気下で1000℃、2時間処理し、炭素
/二酸化珪素のモル比が3.0である二酸化珪素−炭素
複合体を作成した。ZnSe粉末と二酸化珪素−炭素複
合体を、ZnSe60モル%、二酸化珪素−炭素複合体
40モル%(SiO2 10モル%/C30モル%)の混
合比で十分に混合した。この混合粉末をホットプレスを
用いて成型後、直径4インチ、厚さ6mmの円盤状に整
形して本発明のスパッタリングターゲットを作成した。
Example 2 The same porous synthetic quartz glass as in Example 1 was treated at 1000 ° C. for 2 hours in an atmosphere of 100% methane gas to give a silicon dioxide having a carbon / silicon dioxide molar ratio of 3.0. A carbon composite was created. Carbon composites, ZnSe60 mol%, silicon dioxide - - ZnSe powder and silicon dioxide were mixed thoroughly in a mixing ratio of the carbon composite material 40 mol% (SiO 2 10 mol% / C30 mole%). This mixed powder was molded using a hot press and then shaped into a disk having a diameter of 4 inches and a thickness of 6 mm to prepare a sputtering target of the present invention.

【0020】このスパッタリングターゲットを実施例1
と同様にしてバッキングプレートにボンディングしたの
ち、実施例1と同一のスパッタリング装置にセットし
た。スパッタリングチャンバー内部を1.5×10-4P
aまで真空排気したのち、Arガスを2.0×10-1P
aとなるように導入した。RFマグネトロンスパッタリ
ング法により、投入電力400Wでスパッタリングを行
い、基板上にZnSe−Si−O−C薄膜を500nm
形成した。
This sputtering target was used in Example 1.
After bonding to a backing plate in the same manner as above, the same sputtering apparatus as in Example 1 was set. 1.5 × 10 -4 P inside the sputtering chamber
After evacuation to a, Ar gas was 2.0 × 10 -1 P
It was introduced so as to be a. Sputtering was performed with an input power of 400 W by the RF magnetron sputtering method to deposit a ZnSe-Si-O-C thin film on the substrate to 500 nm.
Formed.

【0021】形成された薄膜の組成は、ZnSe60.
4モル%、SiO2 9.8モル%、C29.8モル%で
あり、スパッタリングターゲット組成と極めてよく一致
していた。さらに、同一条件でスパッタリングを繰り返
しても、薄膜の組成はほとんど変動しなかった。
The composition of the formed thin film is ZnSe60.
The content was 4 mol%, SiO 2 was 9.8 mol%, and C was 29.8 mol%, which was in very good agreement with the sputtering target composition. Further, even if the sputtering was repeated under the same conditions, the composition of the thin film hardly changed.

【0022】比較例1 ZnS、SiO2 、C(グラファイト)の粉末をZnS
70モル%、SiO210モル%/C20モル%の混合
比で十分に混合した。実施例1と同様にして、この混合
粉末をホットプレスを用いて成型後、直径4インチ、厚
さ5mmの円盤状に整形してスパッタリングターゲット
を作成した。
Comparative Example 1 ZnS, SiO 2 and C (graphite) powders were mixed with ZnS.
Sufficiently mixed at a mixing ratio of 70 mol%, SiO 2 10 mol% / C 20 mol%. In the same manner as in Example 1, this mixed powder was molded using a hot press and then shaped into a disk shape having a diameter of 4 inches and a thickness of 5 mm to prepare a sputtering target.

【0023】このスパッタリングターゲットを実施例1
と同様にしてバッキングプレートにボンディングしたの
ち、実施例1と同一のスパッタリング装置にセットし
た。実施例1と同様のスパッタリング条件で、スパッタ
リングを行い、基板上にZnS−Si−O−C薄膜を5
00nm形成した。
This sputtering target was used in Example 1.
After bonding to a backing plate in the same manner as above, the same sputtering apparatus as in Example 1 was set. Sputtering was performed under the same sputtering conditions as in Example 1 to form a ZnS-Si-O-C thin film on the substrate.
Was formed to a thickness of 00 nm.

【0024】形成された薄膜の組成は、ZnS82.3
モル%、SiO2 11.5モル%、C6.2モル%であ
り、ZnSとSiO2 との相対比はスパッタリングター
ゲット組成の相対比とほぼ一致しているが、Cはスパッ
タリングターゲット組成比の1/3以下であった。さら
に、同一条件でスパッタリングを繰り返したところ、ス
パッタリングレートが低下するとともに、2回目の薄膜
は、C7.1モル%、3回目の薄膜は、C8.6モル%
とCの比率が変動した。
The composition of the formed thin film is ZnS82.3.
Mol%, SiO 2 11.5 mol% and C 6.2 mol%, and the relative ratio of ZnS and SiO 2 is almost the same as the relative ratio of the sputtering target composition, but C is 1 of the sputtering target composition ratio. It was / 3 or less. Furthermore, when sputtering was repeated under the same conditions, the sputtering rate decreased and the second thin film had C7.1 mol% and the third thin film had C8.6 mol%.
And the ratio of C changed.

【0025】[0025]

【発明の効果】本発明のスパッタリングターゲットは、
上述のごとく、酸化物−炭素複合体と、カルコゲン化合
物とを成型してなるものであるために、次のごとき優れ
た効果が得られる。
The sputtering target of the present invention is
As described above, since the oxide-carbon composite and the chalcogen compound are molded, the following excellent effects can be obtained.

【0026】(1)少なくとも、カルコゲン化合物、酸
化物および炭素(C)とを含むスパッタリングターゲッ
トをスパッタリングして薄膜を形成する場合、形成され
た薄膜の組成がターゲットの組成と極めて良く一致す
る。
(1) When a thin film is formed by sputtering a sputtering target containing at least a chalcogen compound, an oxide and carbon (C), the composition of the formed thin film matches the composition of the target very well.

【0027】(2)長期にわたるスパッタリングを行っ
ても、ターゲット表面の組成が変化せず、形成される薄
膜の組成もほとんど変化しない。
(2) Even if sputtering is performed for a long period of time, the composition of the target surface does not change, and the composition of the thin film to be formed hardly changes.

Claims (4)

【特許請求の範囲】[Claims] 【請求項1】少なくとも、カルコゲン化合物、酸化物お
よび炭素(C)を含むスパッタリングターゲットであっ
て、該ターゲットは、酸化物−炭素複合体と、カルコゲ
ン化合物とを成型してなるものであることを特徴とする
スパッタリングターゲット。
1. A sputtering target containing at least a chalcogen compound, an oxide and carbon (C), wherein the target is formed by molding an oxide-carbon composite and a chalcogen compound. Characteristic sputtering target.
【請求項2】カルコゲン化合物がZnS、ZnSe、Z
nTeからなる群より選ばれた少なくとも一種であるこ
とを特徴とする請求項1記載のスパッタリングターゲッ
ト。
2. A chalcogen compound is ZnS, ZnSe, Z.
The sputtering target according to claim 1, which is at least one selected from the group consisting of nTe.
【請求項3】酸化物がSi、Al、Tiからなる群より
選ばれた少なくとも一種の酸化物であることを特徴とす
る請求項1または2記載のスパッタリングターゲット。
3. The sputtering target according to claim 1, wherein the oxide is at least one oxide selected from the group consisting of Si, Al and Ti.
【請求項4】カルコゲン化合物がZnS、酸化物−炭素
複合体がSi−O−C複合体であることを特徴とする請
求項1〜3記載のいずれかであるスパッタリングターゲ
ット。
4. The sputtering target according to claim 1, wherein the chalcogen compound is ZnS and the oxide-carbon composite is Si—O—C composite.
JP24772892A 1992-09-17 1992-09-17 Sputtering target Ceased JPH06101032A (en)